Hypercrosslinked hydrogel as well as preparation method and application thereof

By introducing metal ion-coordination bonds and ion bonds into the hydrogel, the supercrosslinked structure is formed, and combined with carbon materials, the problem of salt ion crystal blockage in high-concentrated brine treatment is solved, and efficient brine interception and evaporation process stability is achieved , has great application potential in optically driven ZLD.

CN118988181APending Publication Date: 2024-11-22SHANGHAI ADVANCED RES INST CHINESE ACADEMY OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411305013.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The prior art has a problem of salt ion crystal blockage during evaporation in the high-concentration brine treatment, resulting in interruption of the evaporation process, and insufficient fixed ion concentration in the hydrogel molecular network cannot effectively intercept high-concentration brine.

Method used

Supercrosslinked hydrogel is used to form a three-dimensional network structure through metal ion-coordination bonds and ion bonds as dynamic crosslinking points, combining carbon materials to improve photothermal performance, and realize effective interception of salt ions and stability of the evaporation process.

Benefits of technology

Effective interception of high-concentrated brine is achieved, the crystallization of salt ions is avoided on the evaporation surface, the evaporation rate and the stability of the evaporator are improved, and the application potential is huge in the light-driven ZLD process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005048884280000061
    Figure BDA0005048884280000061
  • Figure BDA0005048884280000091
    Figure BDA0005048884280000091
  • Figure BDA0005048884280000092
    Figure BDA0005048884280000092
Patent Text Reader

Abstract

The invention provides a super-crosslinking hydrogel as well as a preparation method and application thereof. The hydrogel provided by the invention has a three-dimensional network structure, and metal ion-coordination bonds and ionic bonds are used as dynamic crosslinking points; the ionic bonds are formed by carboxylic acid functional groups and ammonium ions; the metal ion-coordinate bond is formed by a carboxylic acid functional group and a metal ion. The hydrogel is compact in internal network structure, free of holes and low in water content, can effectively intercept high-concentration brine when being applied to purification treatment of the high-concentration brine, has huge application potential in the process of light-driven ZLD, and is beneficial to stably achieving the process of light-driven ZLD.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the fields of material science and wastewater treatment, and in particular to a hyper-crosslinked hydrogel and a preparation method and application thereof. Background Art

[0002] With the development of modern industry, the discharge of saline wastewater has increased dramatically. If it is discharged into the environment without timely treatment, it will endanger various ecological environments. For the treatment of saline wastewater, zero liquid discharge (ZLD) is one of the most attractive ways. The ZLD system can be divided into a concentration system and a crystallization system. The concentration system concentrates the saline wastewater into nearly saturated brine through technologies such as reverse osmosis. Currently, reverse osmosis and multi-stage distillation can be used to achieve this. The crystallization system crystallizes nearly saturated brine through mechanical vapor compression and other technologies to obtain a solid, but the system has high energy consumption. The lack of an efficient and energy-saving crystallization system is a key challenge in ZLD wastewater treatment.

[0003] With increasingly stringent energy-saving and environmental protection regulations, clean energy (such as solar energy and environmental energy) has received widespread attention from all walks of life. In recent years, solar-driven photothermal interfacial water evaporation technology has been studied by a large number of scholars because it can efficiently utilize solar energy to achieve an efficient distillation process driven by green energy. However, in highly concentrated brine, as evaporation proceeds, salt ions will reach supersaturation at the gas / liquid interface and form salts, which will then cover the evaporation surface. This will cause blockage of the water transport pathway and interrupt the evaporation process. To address this problem, some researchers have proposed designing micro-nano structures of photoevaporation materials so that salt ions can diffuse back to the bulk solution (solution to be evaporated) by driving the concentration gradient to avoid the precipitation of salt crystals at the evaporation interface. However, when the bulk solution is also close to saturation as evaporation proceeds, the concentration gradient-driven diffusion return mechanism fails, and existing strategies still cannot avoid crystallization blocking the evaporation surface.

[0004] Hydrogel is a quasi-solid material composed of a three-dimensional cross-linked polymer network and internal water molecules. It is widely used in light-driven interfaces as evaporators due to its unique three-dimensional skeleton structure, special hydrophilicity, and adjustable chemical and physical properties. But at the same time, the uncharged molecular chains in ordinary hydrogels have limited regulation performance on salt ion transport. Previous research has shown that the introduction of fixed ionizable groups in hydrogels can, to a certain extent, achieve the interception of salt ions through electrostatic repulsion, so that the salt ions remain in the solution to be evaporated. However, due to the limited fixed ion concentration in the hydrogel molecular network in the prior art and the excessively high water content, it is not possible to achieve the interception of highly concentrated brine. Summary of the invention

[0005] In view of the above-mentioned shortcomings of the prior art, the object of the present invention is to provide a hyper-crosslinked hydrogel and a preparation method and use thereof, so as to solve the problems in the prior art.

[0006] To achieve the above objectives and other related objectives, the present invention is achieved through the following technical solutions.

[0007] The first aspect of the present invention provides a hyper-crosslinked hydrogel, which has a three-dimensional network structure and uses metal ion-coordination bonds and ionic bonds as dynamic crosslinking points; the ionic bonds are formed by carboxylic acid functional groups and ammonium ions; the metal ion-coordination bonds are formed by carboxylic acid functional groups and metal ions.

[0008] Preferably, the metal ion forming the metal ion-coordination bond comprises a trivalent metal ion.

[0009] Preferably, the trivalent metal ions include Fe 3+ 、Al 3+ and Cr 3+ .

[0010] Preferably, the water content of the hyper-crosslinked hydrogel film is less than 35%, such as 30%, 28%, 25%, 24%, and more preferably 18-28%.

[0011] The water content parameter is a very important parameter. The water content in the saturated swelling state represents the degree of swelling of the hydrogel cross-linked network and is an intuitive method to reflect its degree of cross-linking. Only when the saturated swelling water content is less than 35%, can it be said that the hydrogel molecular chain has formed a hyper-cross-linked structure, thus providing a prerequisite for achieving a high fixed ion concentration in the hydrogel. If the water content is higher than 35%, the total ionic strength in the hydrogel decreases, and salt ions will precipitate when applied to saturated brine, making it impossible to intercept high-concentration brine and thus fail to evaporate smoothly. In fact, if the water content of the hydrogel membrane is too high, its mechanical strength will be too low, making it impossible to achieve large-scale application.

[0012] The second aspect of the present invention provides a method for preparing the hyper-crosslinked hydrogel as described above, comprising the following steps: mixing anionic monomers, cationic monomers and initiators in water to obtain a precursor solution; coating the precursor solution on a substrate and performing cross-linking polymerization to obtain a hydrogel containing ionic cross-linking points; soaking the hydrogel containing ionic cross-linking points in a metal salt solution, and obtaining the hyper-cross-linked hydrogel after the soaking is completed.

[0013] Preferably, the anionic monomer is selected from one or more of β-(acryloyloxy)propionic acid, methacrylic acid and acrylic acid.

[0014] Preferably, the cationic monomer is selected from one or both of dimethylaminoethyl methacrylate and dimethylaminopropyl acrylamide.

[0015] Preferably, the molar ratio of the anionic monomer to the cationic monomer is 4.5 to 7:1. For example, it can be 5:1, 6:1. This ratio range is not set arbitrarily, but is a very important parameter. If the content of the anionic monomer is too low, most of the anions will coordinate with the cationic monomers, resulting in a decrease in the density of the carboxylic acid groups cross-linked with the metal ions, resulting in a decrease in the metal ion-coordination bonds, thereby affecting the degree of cross-linking and reducing the salt blocking performance; if the content of the anionic monomer is too high, the degree of cross-linking will be too high, the hydrogel network will be too dense, and the escape of water molecules will be hindered, which will lead to a decrease in the evaporation rate. Only within this range can good salt blocking ability be achieved while having a high evaporation rate.

[0016] Preferably, the mass of the initiator is 1-3% of the sum of the mass of the anionic monomer and the cationic monomer. For example, it can be 1%, 2%, or 3%. The initiator is added to initiate a cross-linking polymerization reaction to form a polymer hydrogel network. Only within this range can the anionic / cationic monomers be induced to generate free radicals, and the chain length of the formed polymer is guaranteed to be within a certain range. If there is too much initiator, the polymer chain will be shorter and a network structure cannot be formed.

[0017] Preferably, the concentration of the metal salt solution is 0.01 to 0.3 mol / L. The concentration parameters of the metal salt solution will affect the formation process of the metal ion-ligand bond. If the concentration of the metal salt solution is too high, if it reaches more than 0.3 mol / L, it will cause the external cross-linking of the hydrogel membrane to be too fast, affecting its internal cross-linking, and it is impossible to ensure the structural uniformity of the hydrogel internal; if it is not immersed in the metal salt solution or the concentration of the metal salt solution is too low, it is impossible to further improve the cross-linking degree of the hydrogel membrane, affecting the salt blocking performance.

[0018] The present invention does not specifically limit the amount of water added, as long as it can ensure that the components in the precursor solution can be evenly dispersed without agglomeration or caking. For example, the amount of water added can be 1.5 mL, 2.5 mL, 5 mL, 10 mL, etc.

[0019] Preferably, the initiator comprises one or more of ammonium persulfate and potassium persulfate.

[0020] Preferably, the ratio of the hydrogel containing ionic crosslinking points to the metal salt solution is 13-20:1, g / L, such as 13-16:1, g / L or 16-20:1, g / L.

[0021] Preferably, the metal salt solution comprises a trivalent metal salt solution. Trivalent metal salt ions are more conducive to forming stable metal ion-coordination bond crosslinking points.

[0022] More preferably, the trivalent metal salt solution comprises one or more of a ferric chloride solution, an aluminum chloride solution and a chromium chloride solution.

[0023] Preferably, carbon material may be added to the precursor solution to make the hyper-crosslinked hydrogel film have photothermal properties, so that it can effectively absorb light energy and convert it into heat energy to promote the evaporation process.

[0024] Preferably, the carbon material includes one or more of graphene oxide, carbon nanotubes and nano carbon black.

[0025] Preferably, the mass ratio of the carbon material to water is less than or equal to 0.02:1, such as 0.01:1, 0.012:1, or 0.015:1, so that the carbon material can be evenly dispersed in the system.

[0026] Preferably, the cross-linking polymerization method includes one or both of photopolymerization and thermal polymerization.

[0027] More preferably, the photopolymerization conditions include: irradiation in an ultraviolet environment for 10 to 12 hours.

[0028] More preferably, the conditions for the thermal polymerization include: a heating temperature of 75 to 85° C. and a heating time of 3 hours.

[0029] Preferably, the immersion time is not less than 24 hours, so that the metal ions can fully associate and coordinate with the carboxylic acid groups to form metal ion-coordination bonds as crosslinking points.

[0030] Preferably, after obtaining the hyper-crosslinked hydrogel, it is soaked in water for at least 1 day to remove the uncrosslinked anionic and cationic monomers or metal ions on the surface of the hyper-crosslinked hydrogel.

[0031] In a third aspect, the present invention provides a use of the hyper-crosslinked hydrogel as described above as an evaporator of a light-driven interface in the field of light-driven high-concentration brine zero liquid discharge (ZLD) sewage treatment, wherein the hyper-crosslinked hydrogel is a hyper-crosslinked hydrogel film having a thickness of 0.1 to 0.6 mm, such as 0.1 mm, 0.2 mm, 0.3 mm, 0.4 mm, 0.5 mm, 0.6 mm, and more preferably 0.3 mm.

[0032] Preferably, the highly concentrated brine comprises a sodium chloride solution with a concentration of 20-30 wt%. For example, the concentration of the highly concentrated brine may be 20-26.5 wt%, 26.5-30 wt%.

[0033] Preferably, when used as an evaporator of a light-driven interface, the light intensity is 1 kW / m 2 When the evaporation rate is greater than or equal to 2.5 kg m -2 h-1 .

[0034] Preferably, when treating highly concentrated brine, the hypercrosslinked hydrogel film is exposed to standard sunlight (1 kW / m 2 ) and can operate stably without crystalline salt precipitation on the surface for no less than 8 hours.

[0035] In the technical solution of the present invention, the covalent chemical cross-linking method used in the traditional preparation of hydrogels is abandoned, and no cross-linking agent is used. The traditional covalent cross-linking method relies on specific groups on the molecular chain to form covalent bonds to cross-link different molecular chains. It is affected by steric hindrance and group density, and it is difficult to form a hyper-cross-linked structure, so it is impossible to provide an effective high fixed ion concentration for blocking salt. Metal ion-coordination bonds and ionic bonds are used as dynamic cross-linking points, and the ionic groups carried by each monomer can be used for physical cross-linking. The cross-linking points are abundant, so the construction of a hyper-cross-linked network hydrogel film can be realized, which has excellent salt blocking performance, can effectively prevent salt from being precipitated, and allows the evaporation process to proceed smoothly.

[0036] Specifically, in the present application, cationic monomers and anionic monomers are randomly copolymerized under the initiation of an initiator to form a long polymer chain, wherein the fixed anions (COO - ) and fixed cations (NH 4+ ) are associated with each other through ionic bonds to form a gel network with dynamic cross-linking points to prevent the collapse of the gel structure; then, the gel is immersed in a metal salt solution to introduce metal ions as coordination ions to release some NH 4+ With COO - The ionic bond formed by COO - Re-coordinate with metal ions to form metal ion-coordination bonds as cross-linking points, replacing weak cross-linking points with strong cross-linking points, thereby forming a super cross-linked network hydrogel. In this application, the role of introducing metal ions is to provide empty electron orbitals to interact with COO in the gel network. - Form coordination and cross-linking points; at the same time, the small size and easy penetration of metal ions are used to combine with the rich COO - , which can further increase the cross-linking point density of the gel network to super cross-linking.

[0037] The beneficial effects of the technical solution of the present invention are:

[0038] The hyper-cross-linked hydrogel provided by the technical solution of the present invention has a dense and non-porous internal network structure and a low water content. When applied to the purification of highly concentrated brine, it can effectively retain highly concentrated brine without leakage of salt solution into the hydrogel membrane, thereby avoiding the problem of salt ions in the highly concentrated brine reaching the surface of the hydrogel membrane and then crystallizing; and the hydrogel membrane can operate stably for a long time as an evaporator without crystallized salt precipitation on the surface, which can effectively avoid salt formation at the gas / liquid interface and block the evaporation surface and thus hinder the continuous evaporation process; the technical solution of the present invention has great application potential in the process of light-driven ZLD, and is conducive to the stable realization of the light-driven ZLD process. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 Shown is a schematic diagram of the structure of the hyper-crosslinked hydrogel provided by the present invention.

[0040] Figure 2 Shown is a scanning electron microscope image of the hyper-crosslinked hydrogel film prepared in Example 2 of the present invention.

[0041] Figure 3 Shown is the Fourier infrared spectrum of the hyper-crosslinked hydrogel film prepared in Example 2 of the present invention.

[0042] Figure 4 Shown is the X-ray photoelectron spectroscopy (XPS) of the hyper-crosslinked hydrogel film prepared in Example 2 of the present invention.

[0043] Figure 5 Shown is an energy dispersive X-ray spectrometer (EDS) image of the hyper-crosslinked hydrogel film prepared in Example 2 of the present invention.

[0044] Figure 6 Shown is a graph showing the contact angle test results of the hyper-crosslinked hydrogel film prepared in Example 2 of the present invention.

[0045] Figure 7 Shown is the rheological diagram of the hyper-crosslinked hydrogel film prepared in Example 2 of the present invention.

[0046] Figure 8 The graph shows the swelling rate of the hyper-crosslinked hydrogel film prepared in Example 2 of the present invention in a nearly saturated sodium chloride solution (26.5 wt %).

[0047] Fig. 9 The differential scanning calorimeter (DSC) diagrams of the hydrogel films prepared in Example 2 of the present invention and Comparative Examples 1-2 are shown.

[0048] Fig.10 The graph shows the evaporation rate of the hyper-crosslinked hydrogel film prepared in Example 2 of the present invention in a nearly saturated sodium chloride solution (26.5 wt %). DETAILED DESCRIPTION

[0049] The following is a description of the implementation of the present invention by means of specific embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification.

[0050] Before further describing the specific embodiments of the present invention, it should be understood that the scope of protection of the present invention is not limited to the specific embodiments described below; it should also be understood that the terms used in the examples of the present invention are intended to describe specific embodiments, rather than to limit the scope of protection of the present invention. The test methods in the following examples without specifying specific conditions are generally carried out under conventional conditions or under conditions recommended by the manufacturers.

[0051] When the embodiments give numerical ranges, it should be understood that, unless otherwise specified in the present invention, both endpoints of each numerical range and any numerical value between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those generally understood by those skilled in the art. In addition to the specific methods, equipment, and materials used in the embodiments, according to the grasp of the prior art by those skilled in the art and the record of the present invention, any methods, equipment, and materials of the prior art similar or equivalent to the methods, equipment, and materials described in the embodiments of the present invention can also be used to realize the present invention.

[0052] Taking the anionic monomer as β-(acryloyloxy) propionic acid (CEA) and the cationic monomer as dimethylaminoethyl methacrylate (DMAEMA), and soaking in ferric chloride solution as an example, the preparation flow chart of the hyper-crosslinked hydrogel is as follows:

[0053]

[0054] Example 1

[0055] This embodiment provides a specific hyper-crosslinked hydrogel, wherein the anionic monomer is β-(acryloyloxy) propionic acid (CEA), and the cationic monomer is dimethylaminoethyl methacrylate (DMAEMA), and the preparation steps are as follows:

[0056] 1) 6 g of anionic monomer β-(acryloyloxy) propionic acid (CEA) and 1.3 g of cationic monomer dimethylaminoethyl methacrylate (DMAEMA) (molar ratio 5:1) were added to 2.5 mL of deionized water, stirred for 60 min, nitrogen was passed through for 30 min, and then 0.073 g of initiator ammonium persulfate (1% of the total mass of anionic monomer and cationic monomer) was added to obtain a precursor solution;

[0057] 2) applying the precursor solution onto a glass substrate using a doctor blade, and placing the solution in a UV cross-linking apparatus for cross-linking polymerization for 12 hours to obtain a hydrogel film containing ionic cross-linking points;

[0058] 3) 8 g of the hydrogel film containing ionic crosslinking points was soaked in 500 mL of 0.3 mol / L ferric chloride solution for 24 h, and then the iron ions not involved in the crosslinking were washed away with deionized water, and the deionized water was replaced every 4 h, and the super-crosslinked hydrogel film was obtained.

[0059] Example 2

[0060] This embodiment provides a specific hyper-crosslinked hydrogel with photothermal properties, wherein the anionic monomer is β-(acryloyloxy) propionic acid (CEA), and the cationic monomer is dimethylaminoethyl methacrylate (DMAEMA). The preparation steps are as follows:

[0061] 1) 0.03 g of graphene oxide was added to 2.5 mL of deionized water and stirred for 10 min to obtain a graphene oxide aqueous solution;

[0062] 2) 6 g of anionic monomer β-(acryloyloxy) propionic acid (CEA) and 1.3 g of cationic monomer dimethylaminoethyl methacrylate (DMAEMA) (molar ratio 5:1) were added to 2.5 mL of graphene oxide aqueous solution, stirred for 60 min, nitrogen was passed through for 30 min, and then 0.073 g of initiator ammonium persulfate (1% of the total mass of anionic monomer and cationic monomer) was added to obtain a precursor solution;

[0063] 3) using a doctor blade to apply the precursor solution onto a glass substrate, and placing the solution in a UV cross-linking apparatus for cross-linking polymerization for 12 hours to obtain a hydrogel film containing ionic cross-linking points;

[0064] 4) 8 g of the hydrogel film containing ionic crosslinking points was soaked in 500 mL of 0.3 mol / L ferric chloride solution for 24 h, and then the iron ions not involved in the crosslinking were washed away with deionized water. The deionized water was replaced every 4 h and soaked for 24 h to obtain the super crosslinked hydrogel film.

[0065] The applicant has carried out morphological observation and molecular structure confirmation on the hyper-crosslinked hydrogel film with photothermal properties prepared in this embodiment. Specifically, the applicant has carried out scanning electron microscopy observation, infrared spectrum analysis, X-ray photoelectron spectroscopy (XPS) analysis, and energy dispersive X-ray spectrometer (EDS) analysis on the hyper-crosslinked hydrogel film. The specific results are shown in Figures 2 to 5 Among them, the scanning electron microscope observation experiment used Zeiss Sigma 300; the infrared spectrum analysis used Perkin-Elmer Spectrum GX; the XPS used Thermo Kalpha, and the EDS analysis used Zeiss Sigma 300.

[0066] Depend on Figure 2It can be seen that the internal network structure of the hydrogel membrane is dense and non-porous. Therefore, when it is used as an evaporator, the salt solution will not enter the interior, so the salt ions can be effectively retained.

[0067] Depend on Figure 3 It can be seen that at 1700cm -1 and 1400cm -1 The characteristic peak of carboxylate appeared at 1200 cm -1 NH appeared nearby 4+ This indicates that carboxylic acid and iron ions form carboxylate salts in the hydrogel film, proving that the two are successfully coordinated. Specifically, since only specific Fe 3+ , so COO - The group is at 1700cm -1 and 1400cm -1 The peak at is COO - with Fe 3+ The characteristic peaks of the formed carboxylate salts confirm the existence of metal ion-ligand bonds. In addition, at 1200 cm -1 The characteristic peak nearby is (CH3)3N + The vibration of the CN bond in (CH3)3N + The groups become free, characteristic peaks appear, and the formation of metal-coordination bonds can be confirmed.

[0068] Depend on Figure 4 (XPS) shows that the oxygen atoms in the carboxylic acid (the line formed by the triangle in the figure) have a peak at 530.7 eV, which indicates that the Fe-OC metal ligand bond is formed in the hydrogel film, further confirming that the Fe 3+ With COO - The coordination bond is formed.

[0069] exist Figure 5 In the figure, the dot-shaped particles represent the position distribution of iron elements in the hydrogel film. Figure 5 It can be seen that the iron ions are evenly distributed in the hydrogel film, which indicates that the hydrogel film has uniform performance.

[0070] The applicant also conducted a performance test on the hyper-crosslinked hydrogel film with photothermal properties prepared in this embodiment.

[0071] Contact angle test:

[0072] The contact angle test was performed using Dataphysics OCA20. The wetted hydrogel film was made into a 2×2 cm 2Make sure the two sides of the test sample are flat and smooth, and make sure the top surface is parallel to the test baseline. Drop a 5μL water droplet on the sample surface and measure the angle between the water droplet and the test baseline. Figure 6 .

[0073] Depend on Figure 6 It can be seen that the contact angle between the water droplet and the hydrogel film is 48.02 degrees, which is less than 90 degrees, indicating that the hyper-cross-linked hydrogel film prepared in this example has good hydrophilicity.

[0074] Dynamic rheological testing:

[0075] The rheological test instrument was HAAKE MARS60. The wet hydrogel film was cut into a circle with a diameter of 2.5 cm. A parallel plate rotor was used and the mode was set to oscillation mode. The test frequency range was 0.01-100 rad / s. The specific results are shown in Figure 7 .

[0076] exist Figure 7 In the equation, G' represents the elastic modulus and G" represents the viscous modulus. Figure 7 It can be seen that the elastic modulus is higher than the viscous modulus, which indicates that the morphology of the hydrogel film obtained in Example 2 is quasi-solid. 6 Pa, indicating that the gel network in the hydrogel film is more entangled, and the gel exhibits better elasticity and excellent mechanical properties.

[0077] Swelling rate experiment in saturated salt solution:

[0078] Sodium chloride was added to 80 mL of deionized water until it stopped dissolving. After standing for 30 min, 50 mL of the supernatant was taken to obtain a nearly saturated sodium chloride solution. The dried hydrogel film (thickness 0.3 mm, length and width 1 cm) was then placed in the nearly saturated sodium chloride solution. The hydrogel film was taken out every 180 s, the surface water was wiped off, and the mass of the hydrogel film was weighed to calculate the water content of the hydrogel film and evaluate the swelling condition of the hydrogel film. The specific results are shown in Figure 8 .

[0079] Depend on Figure 8 It can be seen that the hydrogel film (thickness 0.3 mm, length and width 1 cm) prepared in this example can reach saturation equilibrium in 500 seconds in a saturated sodium chloride solution (26.5 wt%). This shows that the hydrogel film prepared in this example can quickly reach swelling equilibrium even in a saturated sodium chloride solution, which is due to the osmotic pressure generated by the high ionic strength inside, which can quickly replenish water molecules.

[0080] Example 3

[0081] This embodiment provides a specific hyper-crosslinked hydrogel with photothermal properties, wherein the anionic monomer is β-(acryloyloxy) propionic acid (CEA), and the cationic monomer is dimethylaminoethyl methacrylate (DMAEMA). The preparation steps are as follows:

[0082] 1) is exactly the same as step 1) of Example 2;

[0083] 2) is exactly the same as step 2) of Example 2;

[0084] 3) is exactly the same as step 3) of Example 2;

[0085] 4) Except that the concentration of the ferric chloride solution is 0.2 mol / L, the remaining steps are exactly the same as step 4) of Example 2.

[0086] Comparative Example 1

[0087] This comparative example provides a specific hydrogel with photothermal properties, wherein the anionic monomer is β-(acryloyloxy) propionic acid (CEA), and the cationic monomer is dimethylaminoethyl methacrylate (DMAEMA). The preparation steps are as follows:

[0088] 1) is exactly the same as step 1) of Example 2;

[0089] 2) except adding 6 g of CEA and 1.63 g of DMAEMA so that the molar ratio is 4:1 and the mass of the initiator ammonium persulfate added is 0.076 g, the remaining steps are exactly the same as step 2) of Example 2;

[0090] 3) is exactly the same as step 3) of Example 2;

[0091] 4) is exactly the same as step 4) of Example 2.

[0092] Comparative Example 2

[0093] This comparative example provides a specific hydrogel with photothermal properties, wherein the anionic monomer is β-(acryloyloxy) propionic acid (CEA), and the cationic monomer is dimethylaminoethyl methacrylate (DMAEMA). The preparation steps are as follows:

[0094] 1) is exactly the same as step 1) of Example 2;

[0095] 2) except adding 6 g of CEA and 2.17 g of DMAEMA so that the molar ratio is 3:1, and the mass of the initiator ammonium persulfate added is 0.082 g, the remaining steps are exactly the same as step 2) of Example 2;

[0096] 3) is exactly the same as step 3) of Example 2;

[0097] 4) is exactly the same as step 4) of Example 2.

[0098] Comparative Example 3

[0099] This comparative example provides a specific hydrogel with photothermal properties, which is prepared in exactly the same manner as in Example 2, except that in step 4), the prepared hydrogel film containing ionic crosslinking points is directly immersed in deionized water for 24 hours to reach swelling equilibrium.

[0100] The applicant measured the water content of the hydrogel films prepared in Examples 1 to 3 and Comparative Examples 1 to 3.

[0101] The specific method is as follows: after the hydrogel films prepared in Examples 1 to 3 and Comparative Examples 1 to 3 are placed in deionized water for 24 hours, the surface moisture is wiped off, and the mass of the hydrogel film is weighed with an analytical balance with an accuracy of 0.0001 g, which is recorded as m1. The hydrogel film is then placed in an oven at 60° C. and dried for 3 hours, and the mass is taken out, which is recorded as m0. Three parallel samples are taken for each Example and Comparative Example, and the moisture content thereof is calculated according to the moisture content calculation formula (as shown in Formula I below). The specific results are shown in Table 1 below.

[0102]

[0103] Formula Ⅰ.

[0104] Table 1

[0105]

[0106] As can be seen from Table 1, the water content of the super-crosslinked hydrogel provided by the technical solution of the present invention is 24% to 25%, which is much lower than the water content of the hydrogel prepared in Comparative Examples 1 to 3; and as can be seen from Example 2 and Comparative Examples 1 and 2, the water content of the hydrogel film prepared therefrom gradually increases. This shows that the water content of the hydrogel film decreases with the increase of the anionic monomer content, because the metal coordination bonds formed with the iron ions after the anionic monomer content increases are more, thereby making the degree of crosslinking greater, the network in the hydrogel film tighter, and the water content lower. It can be seen from the water content of Example 2 and Comparative Example 3 that the water content of the hydrogel film prepared in Example 2 is much lower than that of Comparative Example 1, which shows that if iron ions are not added, the crosslinking degree of the hydrogel film crosslinked by ionic bonds is low, and the water content is high, indicating that when metal ions are added to form metal-coordinated ionic bonds with carboxylic acids, it is beneficial to increase the degree of crosslinking of the hydrogel network, and the gel network formed is tighter and has a lower water content.

[0107] The applicant also conducted DSC tests on the hydrogel films prepared in Example 2 and Comparative Examples 1 and 2 to further observe the water content therein.

[0108] The specific method is as follows: the instrument used in the DSC test is Mettler Toledo DSC3, 10 mg of the sample is taken, the surface moisture is wiped off, and it is placed in an open Al crucible, the nitrogen flux is 100 mL / min, the heating rate is 2°C / min, and the DSC curve transformation of the test sample and water at -30 to 30°C is obtained. The specific results are shown in Fig. 9 .

[0109] In the DSC result graph, the downward peak at 0°C indicates that the hydrogel contains free water. The larger the peak value, the more free water there is in the hydrogel.

[0110] Depend on Fig. 9 It can be seen that the water content of the hydrogel film prepared in Example 2 (the molar ratio of anionic monomer to cationic monomer is 3:1) is the highest, and the water content of the hydrogel film prepared in Example 2 (the molar ratio of anionic monomer to cationic monomer is 5:1) is the lowest. This shows that the water content of the hydrogel film is related to the molar ratio of anionic monomer to cationic monomer, and within a certain range, the water content decreases with the increase of the anionic monomer content. Since the molar ratio of anionic monomer to cationic monomer affects the degree of crosslinking in the hydrogel film, it is further explained that the water content of the hydrogel film is related to its crosslinking degree. The higher the crosslinking degree in the hydrogel, the lower its water content.

[0111] The applicant used the hydrogels prepared in Example 2 and Comparative Examples 1 to 3 as evaporators and conducted light evaporation experiments thereon.

[0112] The specific process is as follows: a xenon lamp is used to simulate sunlight, and the hydrogel films prepared in the above embodiment and comparative example with a length and width of 3 cm and a thickness of 0.3 mm are respectively taken for light evaporation test, and the light intensity is 1 kW / m 2 , duration is 8h.

[0113] The results show that at a light intensity of 1kW / m 2 In the 8-hour continuous light evaporation experiment, no salt crystals were observed on the surface of the hyper-crosslinked hydrogel film obtained in Example 2, indicating that the film can effectively overcome the problem of traditional hydrogel films that salt forms on the surface in a short period of time and blocks the crystallization process; while the hydrogel films in Comparative Examples 1 to 3 can only maintain operation for a short period of time. After a period of time (3 hours), salt formation was found on their surfaces, thereby blocking the evaporation and crystallization process.

[0114] The applicant also tested the hypercrosslinked hydrogel film prepared in Example 2 in a nearly saturated salt solution (26.5wt% NaCl) at a light intensity of 0.5sun (kW / m 2 ), 0.75sun(kW / m 2 ), 1sun(kW / m 2 ) , the test results are shown in Fig.10 .

[0115] Depend on Fig.10 It can be seen that when the hypercrosslinked hydrogel film prepared in this embodiment is used as an evaporator, under standard light (1sun / kW / m 2 ), its evaporation rate is fast, greater than or equal to 2.5 kg m -2 h -1 ; and with the increase of light intensity, the evaporation rate becomes faster and faster. In addition, in the continuous 8-hour light evaporation experiment, no salt crystal precipitation was observed on the surface of the hyper-crosslinked hydrogel film, indicating that the film can effectively overcome the problem of traditional hydrogel films that salt forms on the surface in a short time and blocks the crystallization process, and has great potential in the application of light-driven ZLD.

[0116] In summary, the hyper-cross-linked hydrogel membrane structure provided by the technical solution of the present invention is non-porous and dense, with low water content, and can effectively intercept salt ions during the evaporation process, thereby avoiding the phenomenon of salt formation of high-concentration salt solutions on the surface of the hydrogel membrane; and the hydrogel membrane can operate stably for a long time as an evaporator, without crystalline salt precipitation on the surface, effectively avoiding salt formation at the gas / liquid interface and clogging the evaporation surface and thus hindering the continuous evaporation process; therefore, the technical solution of the present invention has great application potential in the process of light-driven ZLD.

[0117] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A hyper-crosslinked hydrogel, characterized in that: The super-crosslinked hydrogel has a three-dimensional network structure, and uses metal ion-coordination bonds and ionic bonds as dynamic crosslinking points; the ionic bonds are formed by carboxylic acid functional groups and ammonium ions; and the metal ion-coordination bonds are formed by carboxylic acid functional groups and metal ions.

2. The hypercrosslinked hydrogel according to claim 1, characterized in that The metal ions forming the metal ion-coordination bond include trivalent metal ions; And / or, the water content of the hyper-crosslinked hydrogel is <35%.

3. The hypercrosslinked hydrogel according to claim 2, characterized in that The trivalent metal ions include Fe 3+ 、Al 3+ and Cr 3+ One or more of .

4. A method for preparing a hypercrosslinked hydrogel according to any one of claims 1 to 3, characterized in that: The steps include: mixing anionic monomers, cationic monomers and initiators in water to obtain a precursor solution; The precursor solution is coated on a substrate and then cross-linked and polymerized to obtain a hydrogel containing ionic cross-linking points; The hydrogel containing ionic bond cross-linking points is immersed in a metal salt solution, and the super-cross-linked hydrogel is obtained after the immersion is completed.

5. The preparation method according to claim 4, characterized in that: The anionic monomer is selected from one or more of β-(acryloyloxy)propionic acid, methacrylic acid and acrylic acid; And / or, the cationic monomer is selected from one or both of dimethylaminoethyl methacrylate and dimethylaminopropyl acrylamide; and / or, the molar ratio of the anionic monomer to the cationic monomer is 4.5 to 7:1; And / or, the mass of the initiator is 1 to 3% of the sum of the mass of the anionic monomer and the cationic monomer; And / or, the initiator includes one or more of ammonium persulfate and potassium persulfate.

6. The preparation method according to claim 4, characterized in that: The ratio of the hydrogel containing ionic crosslinking points to the metal salt solution is 13 to 20:1, g / L; and / or, the concentration of the metal salt solution is 0.01 to 0.3 mol / L; and / or, the metal salt solution comprises a trivalent metal salt solution; And / or, carbon material may be added to the precursor solution.

7. The preparation method according to claim 6, characterized in that: The trivalent metal salt solution includes one or more of a ferric chloride solution, an aluminum chloride solution, and a chromium chloride solution; And / or, the carbon material includes one or more of graphene oxide, carbon nanotubes and nano carbon black; And / or, the mass ratio of the carbon material to water is less than or equal to 0.02:

1.

8. The preparation method according to claim 4, characterized in that: The cross-linking polymerization method includes one or both of photopolymerization and thermal polymerization; And / or, the soaking time is not less than 24 hours; And / or, after obtaining the hyper-crosslinked hydrogel, the hydrogel is soaked in water for a period of not less than 1 day.

9. Use of the hyper-crosslinked hydrogel as claimed in any one of claims 1 to 3 as an evaporator of a light-driven interface in the field of light-driven high-concentration brine zero liquid discharge sewage treatment.

10. The use according to claim 9, characterized in that The hyper-crosslinked hydrogel is a hyper-crosslinked hydrogel film, and its thickness is 0.1-0.6 mm; And / or, the highly concentrated brine comprises a sodium chloride solution having a concentration of 20 to 30 wt%; and / or, as an evaporator for a light-driven interface, at a light intensity of 1 kW / m 2 When the evaporation rate is greater than or equal to 2.5kgm - 2 h -1 ; And / or, when treating highly concentrated brine, the hyper-crosslinked hydrogel membrane can operate stably under standard sunlight without crystalline salt precipitation on the surface for a period of not less than 8 hours.