Phase change microcapsule and preparation method thereof

Phase change microcapsules were prepared by oxidation-reduction initiated polymerization, which solved the problems of monomer volatilization loss and core material leakage, and achieved higher reaction rate and microcapsule stability.

CN118988186APending Publication Date: 2024-11-22CASIC DEFENSE TECH RES & TEST CENT
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411076840.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing phase change microcapsule encapsulation processes are prone to monomer volatilization loss, resulting in raw material waste and microcapsule core material leakage, and the reaction rate is low.

Method used

The oxidation-reduction initiation polymerization method is adopted. The monomer, crosslinking agent and benzoyl peroxide are dissolved in paraffin, mixed and sheared with aqueous solution to form paraffin emulsion. Then, a reducing agent is added to carry out free radical polymerization, and the reaction temperature is controlled at 70-90℃.

Benefits of technology

It effectively reduced monomer volatilization and heat loss, improved reaction efficiency, and enhanced the stability of microcapsules and monomer conversion rate, increasing it from 50% to 90%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988186A_ABST
    Figure CN118988186A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of phase change microcapsules, in particular to a phase change microcapsule and a preparation method thereof.The preparation method comprises the following steps that S1, a monomer, a cross-linking agent and dibenzoyl peroxide (BPO) are dissolved in paraffin, and an oil phase solution is obtained; the paraffin is No.25 paraffin; s2, adding a water-soluble emulsifier into water, and adjusting the pH value to weak acidity to obtain a water-phase solution; s3, mixing the oil phase solution and the water phase solution, and shearing to obtain a paraffin emulsion; and S4, adding a reducing agent into the paraffin emulsion, carrying out redox polymerization, heating to 70-90 DEG C, and carrying out free radical polymerization. The problems that when an existing phase change microcapsule is coated, monomer volatilization loss is easily caused, so that raw materials are wasted, even the coating degree is affected, a microcapsule core material leaks, and the reaction rate is low are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of phase change microcapsules, in particular to a phase change microcapsule and a preparation method thereof. Background Art

[0002] As people's living standards continue to improve, the requirements for environmental comfort are also getting higher and higher, and the temperature control is also required to be more intelligent and more precise. At the same time, the problem of energy shortage and scarcity is becoming increasingly prominent at this stage. How to use energy efficiently and economically has become a technical problem that needs to be solved urgently in this field;

[0003] Phase change materials use the heat absorption and release of certain substances during the phase change process to store thermal energy and control temperature. Due to its large latent heat of phase change and constant temperature during operation, as well as its ability to weaken external temperature fluctuations, it is widely used in clothing, energy-saving buildings, cold chain logistics and other fields.

[0004] Common phase change energy storage materials include hydrated inorganic salts, fatty acids, paraffin, etc. Among them, paraffin has attracted much attention due to its wide range of phase change temperatures, low cost, large thermal enthalpy, and small supercooling. However, paraffin will undergo physical changes during the melting process, and there is a problem of leakage. Therefore, the use of microencapsulation technology to encapsulate paraffin is more conducive to expanding its application range.

[0005] Polymethyl methacrylate (PMMA), also known as organic glass, has the characteristics of low density and high mechanical strength. It is used as a coating polymer in the field of phase change microcapsules. The coating method in the prior art is to use thermally initiated polymerization. Although the polymerization rate is fast and the coating effect is good, because the initiation temperature is much higher than room temperature, it is easy to cause monomer volatilization loss, resulting in waste of raw materials and even affecting the degree of coating, causing leakage of microcapsule core materials; while the oxidation-reduction initiated polymerization method is to use the free radicals generated by the electron transfer between the oxidant and the reductant to initiate the polymerization reaction. This method can be carried out at a lower temperature and has the advantage of a fast initiation rate. Although it can reduce monomer volatilization to a certain extent to avoid waste of raw materials, it has the problem of low reaction rate. Summary of the invention

[0006] The technical problem to be solved by the present invention is that the existing phase change microcapsules are prone to cause monomer volatilization loss during coating, which leads to a waste of raw materials and even affects the degree of coating, causing leakage of microcapsule core materials, and has a low reaction rate.

[0007] In order to solve the above problems, the technical solution adopted by the present invention is a phase change microcapsule and a preparation method thereof, wherein the preparation method comprises the following steps:

[0008] S1: dissolving the monomer, the cross-linking agent and dibenzoyl peroxide (BPO) in paraffin to obtain an oil phase solution; the paraffin is No. 25 paraffin;

[0009] S2: adding a water-soluble emulsifier to water and adjusting the pH to weak acidity to obtain an aqueous phase solution;

[0010] S3: mixing the oil phase solution and the water phase solution and then shearing them to obtain a paraffin emulsion;

[0011] S4: adding a reducing agent into the paraffin emulsion, and after redox polymerization, heating to 70-90° C. to perform free radical polymerization.

[0012] As a further solution of the present invention: the monomer in S1 is a methacrylic monomer or a styrene monomer, mainly one or more of methyl methacrylate, styrene, n-butyl methacrylate, and tert-butyl methacrylate; the cross-linking agent is selected from one or two of ethylene glycol dimethacrylate (EGDMA) and divinylbenzene; as a preferred technical solution of the present invention, the monomer is selected from methyl methacrylate (MMA) and the cross-linking agent is selected from ethylene glycol dimethacrylate.

[0013] As a further solution of the present invention: the mass ratio of monomer: cross-linking agent: dibenzoyl peroxide: paraffin is in the range of 45-55:45-55:0.5-2:450-550. As a preferred technical solution of the present invention, the ratio of monomer: cross-linking agent: dibenzoyl peroxide: paraffin is 50:50:1:500.

[0014] As a further embodiment of the present invention: the water-soluble emulsifier in S2 is a hydrolyzed styrene-maleic anhydride copolymer; the hydrolyzed styrene-maleic anhydride copolymer is prepared by a method comprising the following steps:

[0015] 1) adding styrene and maleic anhydride into a solvent, adding azobisisobutyronitrile after dissolving, and performing free radical polymerization at 80-90° C. to obtain a styrene-maleic anhydride copolymer;

[0016] 2) adding the styrene-maleic anhydride copolymer into a sodium hydroxide aqueous solution to carry out a hydrolysis reaction.

[0017] As a further embodiment of the present invention, the molar ratio of styrene to the maleic anhydride is in the range of 0.5-1.5:0.5-1.5, and the preferred ratio is 1:1.

[0018] As a further solution of the present invention: the solvent is selected from one or more of toluene, xylene and trimethylbenzene; azobisisobutyronitrile accounts for 0.3-0.6% of the total mass of the styrene and maleic anhydride; and the hydrolysis reaction is carried out at 75-85° C. for 2.5-3.5 hours.

[0019] As a further solution of the present invention: the shearing in S3 is carried out at 9000-11000 rpm for 8-12 min, and the shearing is carried out at a temperature of 30-40°C.

[0020] As a further embodiment of the present invention: the reducing agent in S4 is selected from one or more of ferrous sulfate heptahydrate (FeSO4·7H2O), triethylenetetramine, tetraethylenepentamine, and sodium sulfite, preferably ferrous sulfate heptahydrate; the molar ratio of the reducing agent to the dibenzoyl peroxide is 0.5-1.5:0.5-1.5, preferably 1:1.

[0021] As a further embodiment of the present invention: the redox polymerization is carried out at 30-40° C. for 3.5-4.5 h, preferably at 35° C. for 4 h.

[0022] Compared with the prior art, the present invention reduces monomer volatilization and heat loss while improving the stability of phase-change microcapsules, thereby greatly improving reaction efficiency.

[0023] Beneficial effects of the present invention:

[0024] (1) The preparation method of the present invention can effectively avoid the leakage of paraffin during the melting process, and the obtained phase change microcapsules are more stable;

[0025] (2) The preparation method of the present invention effectively reduces monomer volatilization and avoids monomer waste, while also greatly improving the reaction rate;

[0026] (3) Compared with the traditional single redox system initiation method, the preparation method of the present invention further improves the monomer conversion rate (from 50% to 90%) while reducing the monomer volatilization loss. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:

[0028] Figure 1 The following is a SEM image of a phase-change microcapsule and a preparation method thereof according to the present invention. DETAILED DESCRIPTION

[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] The present invention provides a technical solution to solve the existing problems raised in the background technology.

[0031] Example

[0032] This embodiment provides a phase change microcapsule (such as Figure 1 The specific preparation method of the phase change microcapsule comprises the following steps:

[0033] S1: Melt 25g of No. 25 paraffin, dissolve 2.5g of MMA, 2.5g of EGDMA, and 0.05g of BPO in the melted No. 25 paraffin to obtain an oil phase solution;

[0034] S2: Add a certain amount of toluene to a three-necked flask equipped with a condenser, a thermometer, and a stirrer, add styrene and maleic anhydride (molar ratio of 1:1) accounting for 10% of the mass of toluene after nitrogen deoxygenation, stir and dissolve at room temperature, add initiator azobisisobutyronitrile (AIBN) accounting for 0.5% of the mass of the monomer (i.e., the total amount of styrene and maleic anhydride), stir evenly mechanically, place the three-necked flask in a constant temperature water bath at 85°C, keep stirring, condense and reflux, continue to pass nitrogen, and when white precipitate is observed, continue the reaction for 4 hours and then stop the reaction, cool the reaction mixture to room temperature and filter, and vacuum dry the obtained white powder at 60°C to obtain styrene-maleic anhydride copolymer;

[0035] S3: adding 10% of the styrene-maleic anhydride copolymer to a 10% sodium hydroxide aqueous solution, stirring and hydrolyzing at 80° C. for 3 h to obtain a light yellow transparent viscous solution (i.e., hydrolyzed styrene-maleic anhydride copolymer);

[0036] S4: taking a certain amount of 10% of the hydrolyzed styrene-maleic anhydride copolymer and adding it to 75g of water, adjusting the pH value thereof to 3-4 with 2M hydrochloric acid to obtain an aqueous phase solution;

[0037] S5: After mixing the oil phase solution and the water phase solution, the system is maintained at 35° C., and shear emulsification is performed at 10000 rpm for 10 min using a high-speed shear emulsifier to obtain a paraffin emulsion;

[0038] S6: The paraffin emulsion is transferred to a three-necked flask placed in a 35°C water bath, mechanically stirred, and nitrogen is passed to deoxygenate; FeSO4·7H2O (with a molar ratio of 1:1 to BPO) is dissolved in a small amount of water, and slowly added dropwise to the three-necked flask using a peristaltic pump, the temperature is kept constant at 35°C, and mechanically stirred. After the addition is completed, the reaction is carried out under a nitrogen atmosphere for 4 hours, the temperature is raised to 80°C for reaction for 2 hours, the system is cooled, filtered, and vacuum dried to obtain phase change microcapsules encapsulating No. 25 paraffin (MMA conversion rate is 90%).

[0039] The present invention and its embodiments are described above, and such description is not restrictive. The drawings show only one embodiment of the present invention, and the actual structure is not limited thereto. In short, if ordinary technicians in the field are inspired by it, without departing from the purpose of the invention, they can design a structure and embodiment similar to the technical solution without creativity, which should belong to the protection scope of the present invention.

Claims

1. A phase change microcapsule and a preparation method thereof, characterized in that: The preparation method comprises the following steps: S1: dissolving monomers, crosslinking agents and dibenzoyl peroxide (BPO) in paraffin to obtain an oil phase solution; S2: adding a water-soluble emulsifier to water and adjusting the pH to weak acidity to obtain an aqueous phase solution; S3: mixing the oil phase solution and the water phase solution and then shearing them to obtain a paraffin emulsion; S4: adding a reducing agent into the paraffin emulsion, and after redox polymerization, heating to 70-90° C. to perform free radical polymerization.

2. A phase change microcapsule and a preparation method thereof according to claim 1, characterized in that: The paraffin in S1 is No. 25 paraffin.

3. A phase change microcapsule and a preparation method thereof according to claim 1, characterized in that: The monomer in S1 is a methacrylic monomer or a styrene monomer, mainly one or more of methyl methacrylate, styrene, n-butyl methacrylate, and tert-butyl methacrylate; the crosslinking agent is selected from one or two of ethylene glycol dimethacrylate (EGDMA) and divinylbenzene.

4. A phase change microcapsule and a preparation method thereof according to claim 1, characterized in that: The mass ratio of the monomer: the cross-linking agent: dibenzoyl peroxide: paraffin is 45-55: 45-55: 0.5-2: 450-550.

5. A phase change microcapsule and a preparation method thereof according to claim 1, characterized in that: The water-soluble emulsifier in S2 is a hydrolyzed styrene-maleic anhydride copolymer; the hydrolyzed styrene-maleic anhydride copolymer is prepared by a method comprising the following steps: 1) adding styrene and maleic anhydride into a solvent, adding azobisisobutyronitrile after dissolving, and performing free radical polymerization at 80-90° C. to obtain a styrene-maleic anhydride copolymer; 2) adding the styrene-maleic anhydride copolymer into a sodium hydroxide aqueous solution to carry out a hydrolysis reaction.

6. A phase change microcapsule and a preparation method thereof according to claim 5, characterized in that: The molar ratio of the styrene to the maleic anhydride is 0.5-1.5:0.5-1.

5.

7. A phase-change microcapsule and a preparation method thereof according to claim 5, characterized in that: The solvent is selected from one or more of toluene, xylene and trimethylbenzene; azobisisobutyronitrile accounts for 0.3-0.6% of the total mass of styrene and maleic anhydride; and the hydrolysis reaction is carried out at 75-85° C. for 2.5-3.5 hours.

8. A phase change microcapsule and a preparation method thereof according to claim 1, characterized in that: The shearing in S3 is performed at 9000-11000 rpm for 8-12 min, and the shearing is performed at a temperature of 30-40°C.

9. A phase-change microcapsule and a preparation method thereof according to claim 1, characterized in that: The reducing agent in S4 is selected from one or more of ferrous sulfate heptahydrate (FeSO4·7H2O), triethylenetetramine, tetraethylenepentamine, and sodium sulfite; the molar ratio of the reducing agent to the dibenzoyl peroxide is 0.5-1.5:0.5-1.5, and the redox polymerization is carried out at 30-40°C for 3.5-4.5h.

10. A phase-change microcapsule and a preparation method thereof according to claims 1-9, the present invention further provides a phase-change microcapsule, Prepared by the above preparation method.