Preparation of blocky attapulgite-based foam material and application of blocky attapulgite-based foam material in adsorption of elemental iodine and iodide ions
Through the preparation of blocky concave and convex rock-based foam materials, the efficient removal and recovery of polyvalent iodine is solved by using N heteroatoms and π-π conjugated bond technology, and the efficient adsorption of iodine ions and the elemental iodine Physical adsorption reduces costs and improves adsorption stability and recovery.
Patent Information
- Application Number
- CN202411301048.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art has high cost, pollution problems and low selective adsorption efficiency when removing polyvalent iodine, especially the poor application effect of traditional porous materials in complex environments.
The blocky concave and convex rock-based foam material is used to adsorb iodine ions through N heteroatoms and to achieve efficient removal of elemental iodine by using π-π conjugated bonds. The macromorphology and size of the material are adjustable to form a three-dimensional network structure. Improve adsorption stability and recovery.
It realizes efficient adsorption and rapid recovery of multivalent iodine, reduces operating costs, avoids secondary pollution, and the material exhibits efficient adsorption performance under different environments.
Smart Images

Figure CN118988247A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sewage purification in environmental protection, and in particular to a preparation method of a blocky polymer foam material using attapulgite as a matrix material and an application thereof in adsorbing elemental iodine and iodide ions. Background Art
[0003] The removal of multivalent iodine has always been a difficult problem. Chemical precipitation, porous material adsorption, ion exchange and membrane separation techniques can be used to remove monovalent radioactive iodine. The metal materials used in chemical precipitation are expensive and easily cause secondary pollution of heavy metals. Due to the use of organic or inorganic solvents, ion exchange technology is also prone to secondary pollution. Although membrane separation technology has good removal efficiency, its operating cost is relatively expensive. Although traditional porous materials have the advantage of low operating costs, it is difficult to guarantee the selective adsorption efficiency in complex environments. Therefore, loading heteroatoms that are selective for target pollutants in porous materials is a good choice.
[0004] Chinese patent CN20211130356.3 uses the N heteroatom of the "shell" in the Yolk-shell composite microsphere to enrich the iodine ions in the solution, and then uses the copper of the "core" to solidify the iodine ions, thereby achieving high-efficiency removal of iodine ions. However, this material is only used for the adsorption of single iodine ions. In Chinese patent CN201910385471.1, hollow composite microspheres with a size of about 30 μm are prepared using diethylaminoethyl methacrylate as a polymerization monomer, ethylene glycol dimethacrylate as a cross-linking agent, and attapulgite as a matrix material. Although the microspheres are large in size, they still have the disadvantages of being difficult to recycle and easy to cause secondary pollution in the actual application of removing pollutants from water bodies. Summary of the invention
[0005] Purpose of the invention: In view of the problems existing in the prior art, the present invention provides a preparation method of a blocky attapulgite-based foam material and its application in adsorbing elemental iodine and iodine ions, utilizing the N heteroatoms in the material to effectively adsorb iodine ions, and then utilizing the π-π conjugated bonds in the material to effectively remove elemental iodine. The macroscopic morphology and size of the material can be adjusted according to the mold during synthesis. Compared with traditional adsorbents, it realizes the adsorption and rapid recovery of multivalent iodine, providing a technical reference for the removal of radioactive multivalent iodine in wastewater.
[0006] Technical solution: In the first aspect, the present invention provides a method for preparing a blocky attapulgite-based foam material, comprising the following steps: S1: pretreating the attapulgite to obtain purified attapulgite; S2: Sodium bisulfite, dimethylaminoethyl methacrylate, polyethylene glycol diacrylate and deionized water are added to the light-transmitting mold respectively and stirred evenly; then, under N2 protection conditions, the purified attapulgite and hexadecyltrimethylammonium bromide are added to the light-transmitting mold, and stirred at high speed to form a foam emulsion; then, ammonium persulfate is added to the foam emulsion, and the mixture is continuously stirred and polymerized under light; S3: taking out the photopolymerized product from the light-transmitting mold, washing it through Soxhlet extraction, and then soaking it in anhydrous ethanol and drying it to obtain a block-shaped attapulgite-based foam material.
[0007] Further, in S1, the specific steps of the attapulgite pretreatment are as follows: The attapulgite clay is soaked in deionized water for 1-2 hours, and then stirred at 8000-9000 r / min for 20-30 minutes to prepare attapulgite slurry, centrifuged, and the upper layer of fine and soft attapulgite is taken and dried to obtain purified attapulgite.
[0008] Furthermore, in S2, the mass ratio of the deionized water, sodium bisulfite, dimethylaminoethyl methacrylate, polyethylene glycol diacrylate, purified attapulgite, hexadecyltrimethylammonium bromide and ammonium persulfate is 1:0.01~0.03:0.1~0.6:0.05~0.2:0.05~0.2:0.01~0.04:0.01~0.04.
[0009] Furthermore, in S2, the specific conditions of the high-speed stirring are: a stirring rate of 3500 to 8000 r / min, and a stirring time of 10 to 330 min.
[0010] Furthermore, in S2, the specific conditions of the photopolymerization are: the photopolymerization temperature is 30 to 50°C, and the photopolymerization time is 10 to 15 h.
[0011] Preferably, in S3, the time of washing by Soxhlet extraction is 10-14 h.
[0012] In a second aspect, the present invention provides an application of a block of attapulgite-based foam material prepared by any of the above methods in absorbing elemental iodine in water, wherein the amount of the block of attapulgite-based foam material added to the water is 0.25-2 g·L -1 ; The adsorption temperature is 25~55 ºC; The adsorption time is 0.08 ~ 12 h.
[0013] In a third aspect, the present invention provides an application of a block of attapulgite-based foam material prepared by any of the above methods in adsorbing iodine ions in water, wherein the amount of the block of attapulgite-based foam material added to the water is 0.25-2 g·L -1; The adsorption pH value is 2 ~6; the adsorption temperature is 25~55 ºC; the adsorption time is 5~30 min.
[0014] In a fourth aspect, the present invention provides an application of a block of attapulgite-based foam material prepared by the method described in any one of the above items in the adsorption of gaseous iodine: the adsorption temperature of the block of attapulgite-based foam material during the adsorption of gaseous iodine is 55~85 ºC, and the adsorption time is 12~36 h.
[0015] Beneficial effects: The present invention uses attapulgite mineral with good stability, low price and large specific surface area as the matrix material, uses alcohol ester containing π-π conjugated bonds as the cross-linking agent, and amino ester as the polymerization monomer, and mixes with attapulgite and a surfactant under the protection of N2 blowing to prepare a foam emulsion, polymerizes under visible light irradiation, uses Soxhlet extraction and washing to remove organic impurities, then soaks in anhydrous ethanol to remove moisture, and finally dries in a supercritical drying device to form a blocky attapulgite-based foam material.
[0016] When the blocky attapulgite-based foam material prepared by the present invention is used to adsorb iodine ions in water, in an acidic environment, the tertiary amine groups in the foam material are protonated and positively charged, and the iodine ions in the solution are attracted by electrostatic attraction. - , while in alkaline environment, the adsorbed I - When the prepared blocky attapulgite-based foam material is used to adsorb elemental iodine in the solution, the π-π conjugated bonds in the foam material have a strong affinity for I2, which can be physically adsorbed in the material. At the same time, the tertiary amine group in the foam material is an electron donor, and iodine is an electron acceptor, so an electron transfer complex can be formed, and the lone pair of electrons on the nitrogen heteroatom is transferred to I2, and N∙∙I2 is converted into N + I - Internal complex, and consumes more I2 to form I3 - , thereby achieving efficient adsorption of elemental iodine.
[0017] Compared with the prior art, the present invention has the following significant advantages: (1) the present method utilizes a mold to prepare a block foam material, and the macroscopic morphology and size of the material can be adjusted according to the mold during synthesis, which is convenient for recycling; (2) the present method utilizes high-speed beating to make the surfactant hexadecyltrimethylammonium bromide form foam, and the high aspect ratio and high adsorption characteristics of attapulgite form a three-dimensional network structure that stably wraps the bubbles formed by high-speed beating for a long time, thereby forming a porous structure after polymerization, making the material more solid, and the material is not easy to split during iodine adsorption, which is convenient for recycling and reuse; (3) the prepared attapulgite-based foam material has the function of simultaneously adsorbing elemental iodine and iodide ions. BRIEF DESCRIPTION OF THE DRAWINGS Figure 1This is a photo of the blocky attapulgite-based foam material after polymerization in Embodiment 1; Figure 2 This is an internal SEM image of a sliced block of attapulgite-based foam material prepared in Embodiment 1; Figure 3 FT-IR spectrum of the blocky attapulgite-based foam material prepared in Embodiment 1; Figure 4 is an adsorption curve of elemental iodine in cyclohexane by the blocky attapulgite-based foam material prepared in Embodiment 1; Figure 5 This is a SEM image of the blocky attapulgite-based foam material prepared in Embodiment 2; Figure 6 is an XRD spectrum of the blocky attapulgite-based foam material prepared in Embodiment 2; Figure 7 is an adsorption curve diagram of the blocky attapulgite-based foam material prepared in Implementation Method 2; Figure 8 These are photos of the blocky attapulgite-based foam material prepared in Embodiment 2 before, during and after adsorption; Fig. 9 This is a SEM image of the blocky attapulgite-based foam material prepared in Embodiment 3; Fig.10 is an XRD spectrum of the blocky attapulgite-based foam material prepared in Embodiment 3; Fig.11 is an adsorption curve diagram of the blocky attapulgite-based foam material prepared in Implementation Method 3; Fig.12 This is a SEM image of the blocky attapulgite-based foam material prepared in Embodiment 4; Fig.13 is an XRD spectrum of the blocky attapulgite-based foam material prepared in Embodiment 4; Fig.14 is an adsorption curve diagram of the blocky attapulgite-based foam material prepared in Implementation Method 4; Fig.15 These are photos of the blocky attapulgite-based foam material prepared in Embodiment 4 before and after adsorption. DETAILED DESCRIPTION
[0019] The present invention is described in detail below in conjunction with the embodiments.
[0020] The specific processing steps of the purified attapulgite in the following embodiment of the present invention are as follows: soaking the attapulgite clay in deionized water for 1 hour, using a high-speed stirrer to stir at 8000 r / min for 30 minutes to make a attapulgite slurry, centrifuging, taking the upper layer of fine soft attapulgite, and drying to obtain attapulgite with non-clay mineral impurities removed, that is, purified attapulgite.
[0021] Implementation 1: 0.1 g of sodium bisulfite, 2 mL of dimethylaminoethyl methacrylate, 0.5 mL of polyethylene glycol diacrylate and 5 mL of deionized water were added to the mold to obtain a mixed solution (in this embodiment, a conventional beaker was used as the mold). Under N2 protection conditions, 0.5 g of purified attapulgite and 0.1 g of hexadecyltrimethylammonium bromide were added to the mixed solution, stirred at 4000 r / min for 10 min using a high-speed stirrer, and finally 0.1 g of ammonium persulfate was added and stirred for another 1 min. The obtained foam was sealed and placed at 40°C for photopolymerization for 12 h, and the obtained product was washed by Soxhlet extraction for 12 h. Finally, the crude product was soaked in anhydrous ethanol for dehydration for 36 h, and then dried for 12 h using a supercritical drying device to obtain a block of attapulgite-based foam material.
[0022] The morphology of the blocky attapulgite-based foam material prepared in this embodiment was observed by SEM. Figure 1 This shows that the overall appearance of the prepared blocky attapulgite-based foam material can be controlled to a centimeter size by the synthetic mold. Figure 2 ) shows the macroporous structure inside the material. FT-IR spectrum ( Figure 3 ) showed that the synthesized sample was composed of attapulgite, polydimethylaminoethyl methacrylate and polyethylene glycol diacrylate.
[0023] 50 mg of the blocky attapulgite-based foam material prepared above was added to 50 mL of a 2 g / L cyclohexane solution of simulated elemental iodine. After open adsorption for 720 min at room temperature, the solution was filtered and the residual elemental iodine concentration in the solution was detected. Figure 4 The adsorption results showed that the blocky attapulgite-based foam material reached adsorption equilibrium within 210 min, with an adsorption capacity of 1.5 g / g and an adsorption efficiency of 75%.
[0024] 1 g of elemental iodine solid was placed at the bottom of the vacuum desiccator, and then 200 mg of the prepared block attapulgite-based foam material was placed on the glass petri dish on the porcelain plate. The desiccator was sealed and placed in a 75°C oven for 24 h. After adsorption, the sample was cooled to room temperature, and the weight of the block attapulgite-based foam material after adsorption was weighed to be 646.8 mg, so the adsorption capacity of the block attapulgite-based foam material was 3.234 g / g.
[0025] Implementation 2: 0.05 g of sodium bisulfite, 0.5 mL of dimethylaminoethyl methacrylate, 0.25 mL of polyethylene glycol diacrylate and 5 mL of deionized water were added to the mold to obtain a mixed solution (in this embodiment, a conventional beaker was used as the mold). Under N2 protection conditions, 0.25 g of purified attapulgite and 0.05 g of hexadecyltrimethylammonium bromide were added to the mixed solution, stirred at 6000 r / min for 30 min using a high-speed stirrer, and finally 0.05 g of ammonium persulfate was added and stirred for another 1 min. The obtained foam was sealed and placed at 40°C for photopolymerization for 10 h, and the obtained product was washed by Soxhlet extraction for 12 h. Finally, the crude product was soaked in anhydrous ethanol for dehydration for 24 h, and then dried for 12 h using a supercritical drying device to obtain a block of attapulgite-based foam material.
[0026] The morphology of the blocky attapulgite-based foam material prepared in this embodiment was observed by SEM. Figure 5 This is a cross-sectional electron microscope image of the blocky attapulgite-based foam material prepared in this embodiment, indicating that the material still has a macroporous structure. FT-IR spectrum ( Figure 6 ) showed that the synthesized sample was composed of attapulgite, polydimethylaminoethyl methacrylate and polyethylene glycol diacrylate.
[0027] 50 mg of the blocky attapulgite-based foam material prepared above was added into 50 mL of 0.5-6.3 g / L cyclohexane solution of simulated elemental iodine, and after open adsorption for 120 min at room temperature, the solution was filtered and the residual elemental iodine concentration in the solution was measured. Figure 7 The adsorption results show that the maximum adsorption capacity of blocky attapulgite-based foam material is 2.14 g / g. Figure 8 Shown are photos of the blocky attapulgite-based foam material before, during and after adsorption of a 1.0 g / L elemental iodine solution. It can be seen that the blocky structure is easily recycled and is not prone to secondary pollution. At the same time, the iodine in the solution is basically completely adsorbed.
[0028] Implementation 3: 0.15 g of sodium bisulfite, 3 mL of dimethylaminoethyl methacrylate, 1 mL of polyethylene glycol diacrylate and 5 mL of deionized water were added to the mold to obtain a mixed solution (in this embodiment, a conventional beaker was used as a mold). Under N2 protection conditions, 1 g of purified attapulgite and 0.2 g of hexadecyltrimethylammonium bromide were added to the mixed solution, stirred at 8000 r / min for 60 min using a high-speed stirrer, and finally 0.2 g of ammonium persulfate was added and stirred for another 1 min. The obtained foam was sealed and placed at 50°C for photopolymerization for 15 h, and the obtained product was washed by Soxhlet extraction for 12 h. Finally, the crude product was soaked in anhydrous ethanol for dehydration for 36 h, and then dried for 12 h using a supercritical drying device to obtain a block of attapulgite-based foam material.
[0029] The morphology of the blocky attapulgite-based foam material prepared in this embodiment was observed by SEM. Fig. 9 This is a cross-sectional electron microscope image of the prepared blocky attapulgite-based foam material after slicing, illustrating the macroporous structure inside the material. FT-IR spectrum ( Fig.10 ) showed that the synthesized sample was composed of attapulgite, polydimethylaminoethyl methacrylate and polyethylene glycol diacrylate.
[0030] 50 mg of the blocky attapulgite-based foam material prepared above was added to 50 mL of a simulated iodide ion solution with an initial concentration of 0.5-10 mM, and the pH value of the solution was adjusted to 2. After open adsorption for 10 min at room temperature, the solution was filtered and the residual iodide ion concentration in the solution was measured. Fig.11 The adsorption results showed that the adsorption capacity of the prepared blocky attapulgite-based foam material was 2.1 mmol / g.
[0031] Implementation 4: 0.1 g of sodium bisulfite, 2 mL of dimethylaminoethyl methacrylate, 0.5 mL of polyethylene glycol diacrylate and 5 mL of deionized water were added to the mold to obtain a mixed solution (in this embodiment, a conventional beaker was used as a mold). Under N2 protection conditions, 0.5 g of purified attapulgite and 0.12 g of hexadecyltrimethylammonium bromide were added to the mixed solution, stirred at 3500 r / min for 330 min using a high-speed stirrer, and finally 0.2 g of ammonium persulfate was added and stirred for another 1 min. The obtained foam was sealed and placed at 30°C for photopolymerization for 12 h, and the obtained product was washed by Soxhlet extraction for 12 h. Finally, the crude product was soaked in anhydrous ethanol for dehydration for 36 h, and then dried for 12 h using a supercritical drying device to obtain a block of attapulgite-based foam material.
[0032] The morphology of the blocky attapulgite-based foam material prepared in this embodiment was observed by SEM. Fig.12 This is a cross-sectional electron microscope image of the prepared blocky attapulgite-based foam material after slicing, illustrating the macroporous structure inside the material. FT-IR spectrum ( Fig.13 ) showed that the synthesized sample was composed of attapulgite, polydimethylaminoethyl methacrylate and polyethylene glycol diacrylate.
[0033] 12.5 mg of the blocky attapulgite-based foam material prepared above was added to 50 mL of a solution containing 0.8 mM I2 (10% methanol solution) and 1.50 mM iodine ions. After adsorption for 10 s, the full wavelength scanning was performed using an ultraviolet spectrophotometer to obtain the following: Fig.14 According to the absorbance at 292 nm and 354 nm, it can be seen that the prepared blocky attapulgite-based foam material has an ultra-high adsorption efficiency for iodine ions and elemental iodine in the mixed solution. Fig.15 These are photos before and after adsorption, which also show that the blocky attapulgite-based foam material basically completely adsorbs elemental iodine and iodine ions.
[0034] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent transformation or modification made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a blocky attapulgite-based foam material, It is characterized in that The following steps are involved: S1: pretreating the attapulgite to obtain purified attapulgite; S2: Sodium bisulfite, dimethylaminoethyl methacrylate, polyethylene glycol diacrylate and deionized water are added to the light-transmitting mold respectively and stirred evenly; then, 2 Under protective conditions, adding the purified attapulgite and hexadecyltrimethylammonium bromide to the light-transmitting mold, stirring at high speed to form a foam emulsion; then adding ammonium persulfate to the foam emulsion, stirring continuously, and polymerizing under light; S3: taking out the photopolymerized product from the light-transmitting mold, washing it through Soxhlet extraction, and then soaking it in anhydrous ethanol and drying it to obtain a block-shaped attapulgite-based foam material.
2. The method for preparing the blocky attapulgite-based foam material according to claim 1, Features: In S1, the specific steps of the attapulgite pretreatment are as follows: The attapulgite clay is soaked in deionized water for 1-2 hours, and then stirred at 8000-9000 r / min for 20-30 minutes to prepare attapulgite slurry, centrifuged, and the upper layer of fine and soft attapulgite is taken and dried to obtain purified attapulgite.
3. The method for preparing the blocky attapulgite-based foam material according to claim 1, Features: In S2, the mass ratio of the deionized water, sodium bisulfite, dimethylaminoethyl methacrylate, polyethylene glycol diacrylate, purified attapulgite, hexadecyltrimethylammonium bromide and ammonium persulfate is 1:0.01~0.03:0.1~0.6:0.05~0.2:0.05~0.2:0.01~0.04:0.01~0.
04.
4. The method for preparing the blocky attapulgite-based foam material according to claim 1, Features: In S2, the specific conditions of the high-speed stirring are: a stirring rate of 3500 to 8000 r / min, and a stirring time of 10 to 330 min.
5. The method for preparing the blocky attapulgite-based foam material according to claim 1, Features: In S2, the specific conditions of light polymerization are: light temperature is 30 ~ 50 ℃, and light time is 10 ~ 15 h.
6. The method for preparing the blocky attapulgite-based foam material according to claim 1, Features: In S3, the Soxhlet extraction and washing time is 10-14 h.
7. Use of a blocky attapulgite-based foam material prepared by the method according to any one of claims 1 to 6 for absorbing elemental iodine in water. Features: The amount of the blocky attapulgite-based foam material added to the water body is 0.25-2 g·L -1 ; The adsorption temperature is 25~55 ºC; The adsorption time is 0.08 ~ 12 h.
8. Use of a blocky attapulgite-based foam material prepared by the method according to any one of claims 1 to 6 for adsorbing iodine ions in water. Features: The amount of the blocky attapulgite-based foam material added to the water body is 0.25-2 g·L -1 ; The adsorption pH value is 2 ~6; the adsorption temperature is 25~55 ºC; the adsorption time is 5~30 min.
9. Use of a blocky attapulgite-based foam material prepared by the method according to any one of claims 1 to 6 in adsorbing gaseous iodine, Features: The adsorption temperature of the blocky attapulgite-based foam material during the adsorption of gaseous iodine is 55-85°C, and the adsorption time is 12-36 h.
Citation Information
Patent Citations
Preparation method of Cu-attapulgite-NH2 composite material and application of Cu-attapulgite-NH2 composite material to adsorption of iodide ions in radioactive water body