Zn-regulated PtSn / Al2O3 catalyst, preparation method and propane dehydrogenation application
Through the Zn-regulated PtSn/Al2O3 catalyst, the problem of poor high temperature stability in the prior art is solved, and the production of propylene with high conversion and high selectivity in the direct propane dehydrogenation reaction is achieved, which improves the long-term stability and economics of the catalyst. sex.
Patent Information
- Application Number
- CN202411066033.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-05
AI Technical Summary
The existing propane direct dehydrogenation catalysts have poor stability under high temperature conditions, resulting in rapid deactivation of the catalyst, affecting the production efficiency and economicality of propylene.
The PtSn/Al2O3 catalyst regulated by Zn is prepared in organic solvents by electrostatic adsorption. The Zn element modification is used to enhance the stability and activity of the catalyst, combining potassium chloroplatinate, stannous chloride and tetrabutyl ammonium bromide. and other raw materials to form efficient catalysts.
Under 600°C, the propane conversion rate of the catalyst remained stable, the propylene selectivity was high, and the conversion rate of the catalyst was almost no decrease within 2000 minutes, which significantly improved the thermal stability and economic benefits of the catalyst.
Smart Images

Figure CN118988302A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of propane dehydrogenation, and specifically relates to a Zn-regulated PtSn / Al2O3 catalyst, a preparation method and an application of propane dehydrogenation. Background Art
[0002] It is a general trend to use traditional basic chemical raw materials to prepare high-end chemicals and new materials and realize the resource conversion of low-value organic matter. Propylene is an important organic basic chemical raw material with a production volume second only to ethylene. It is widely used in the production of chemical products such as polypropylene, acrylonitrile, and propylene oxide. It is the basic raw material of the three major synthetic materials (plastics, rubber, and fibers). The continuous development of the global economy has led to a rapid increase in the demand for propylene. There are four main processes for producing propylene at home and abroad: catalytic cracking technology, steam cracking unit by-product propylene technology, coal or methanol to olefins technology, and propane dehydrogenation technology (PDH technology). At present, the traditional process for producing propylene in China is still petroleum catalytic cracking and naphtha cracking. However, petroleum resources are becoming increasingly scarce and prices are rising. The propylene production technology based on petroleum as raw material urgently needs to be further updated and optimized. At the same time, the development of other propylene production technologies is also imminent. In recent years, the large-scale exploitation of shale gas has effectively increased the production of propane and provided sufficient raw materials for propane dehydrogenation to produce propylene. Propane dehydrogenation is considered to be one of the most promising methods for propylene production.
[0003] Propane catalytic dehydrogenation technology is mainly divided into two categories: oxidative dehydrogenation and direct dehydrogenation according to the different reaction gases. Propane oxidative dehydrogenation technology (OPDH) is to add oxidizing gases (such as nitrogen oxides, carbon dioxide and oxygen, etc.) during the reaction process. The reaction equation of propane oxidative dehydrogenation is as shown in equation (1). When oxygen is used as an oxidizing gas, it breaks the thermodynamic limitation and is an exothermic reaction. The required reaction temperature is low and the energy consumption is low, but propane and the generated propylene are easily oxidized to produce CO or CO2. In recent years, the propane oxidative dehydrogenation reaction has attracted people's attention, and many efficient new metal oxide catalysts have also been developed, such as MnO x 、CoO x and VO x Although the propane oxidative dehydrogenation reaction has high activity, its selectivity for propylene is low, the resulting product distribution is complex and difficult to separate, making it difficult to carry out industrial production, which limits the propane oxidative dehydrogenation reaction to conceptual research.
[0004] C3H8 + O2 → C3H6 + H2O (1)
[0005]
[0006] Compared with OPDH, direct dehydrogenation of propane (PDH) has high selectivity and high yield and has broad industrial application prospects. xThe Pt-based catalyst is used in the commercial PDH process due to its excellent activity and high propylene yield. x The catalyst is safe and environmentally friendly, and is an environmentally friendly catalyst. It has the scientific nature of basic research and has attracted extensive attention from researchers at home and abroad. The direct dehydrogenation (PDH) reaction of propane is shown in equation (2). The reaction temperature is usually between 500 and 600 °C. As an endothermic process, the high temperature environment and harsh conditions severely restrict the development of catalysts. In the dehydrogenation process, side reactions such as cracking, hydrogenolysis and deep dehydrogenation will inevitably occur, forming coke deposition on the catalyst surface, which seriously reduces the activity and stability of the catalyst. For Pt-based catalysts, surface carbon deposition is one of the main reasons for catalyst deactivation. The dehydrogenation reaction of propane on Pt-based catalysts is a structure-insensitive reaction, while side reactions such as cracking, hydrolysis, isomerization and carbon deposition are structure-sensitive reactions. At present, the industrial catalyst widely used in PDH reactions is mainly PtSn / Al2O3. Although the catalyst has good initial activity, its high-temperature thermal stability is still unsatisfactory. It will quickly deactivate in a short time, which not only leads to poor economic benefits, but also causes waste of resources. Summary of the invention
[0007] In order to overcome the problem of poor high-temperature thermal stability of catalysts in the prior art, the purpose of the present invention is to provide a Zn-regulated PtSn / Al2O3 catalyst, a preparation method and an application in propane dehydrogenation. The catalyst prepared by the method has good catalytic activity and excellent high-temperature stability, and can be used in industrial propane dehydrogenation reaction to produce propylene.
[0008] To achieve the above object, the technical solution of the present invention is as follows:
[0009] A method for preparing a Zn-regulated PtSn / Al2O3 catalyst comprises the steps of: placing a metal ion source containing platinum and tin and a Pt-coordinated organic matter in an organic solvent, and adopting an electrostatic adsorption method to prepare the Zn-regulated PtSn / Al2O3 catalyst; the metal ion source containing platinum and tin comprises potassium chloroplatinite and stannous chloride.
[0010] Further, the following steps are included:
[0011] Adding the acid solution of zinc chloride to the potassium chloroplatinite solution, then adding the dichloromethane solution of the Pt coordinated organic matter, separating the layers, and taking the lower layer to obtain a clear solution;
[0012] Adding the tetrahydrofuran solution of stannous chloride to the clear solution, stirring evenly, to obtain a mixed solution;
[0013] Adding a suspension of aluminum oxide in tetrahydrofuran to the mixed solution, stirring to obtain a solid;
[0014] The solid is dried and calcined to obtain a Zn-regulated PtSn / Al2O3 catalyst.
[0015] Furthermore, the molar ratio of zinc chloride, potassium chloroplatinite and stannous chloride is (0.1-0.7):1:(1-5).
[0016] Furthermore, the Pt coordinated organic compound is tetrabutylammonium bromide.
[0017] Furthermore, the mass ratio of the Pt coordinated organic matter to potassium chloroplatinite is 10.0-30.0:10.0-20.0.
[0018] Furthermore, the mass ratio of aluminum oxide to potassium chloroplatinite is 0.600:10.0-20.0.
[0019] Furthermore, the calcination temperature is 500-600°C and the calcination time is 1-3h.
[0020] Furthermore, calcination is carried out under a mixture of H2 and Ar; the temperature is increased to 500-600°C at a heating rate of 5-10°C / min.
[0021] A Zn-regulated PtSn / Al2O3 catalyst, wherein the catalyst is a metal cluster with a size of 1-2 nm.
[0022] Application of a Zn-regulated PtSn / Al2O3 catalyst in propane dehydrogenation.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] In the present invention, a metal ion source containing platinum and tin and a Pt-coordinated organic matter are prepared in an organic solvent by an electrostatic adsorption method. The Zn element is used for modification, which greatly improves the stability of the catalyst. The catalyst has a high conversion rate and maintains excellent stability. Compared with other preparation methods, this method not only shortens the synthesis time, but also has simple equipment requirements, saving time and energy. At the same time, the raw material price is low, the sample has a regular microstructure, high activity, excellent thermal stability and extremely high propylene selectivity, and has a high reference and research value for industrial propane dehydrogenation reaction to produce propylene.
[0025] When the catalyst of the present invention is used in a propane dehydrogenation reaction, propane is adsorbed on the catalyst surface and combined with the activity, the primary carbon bond of propane is broken and a hydrogen atom is shed, and then the secondary carbon bond is broken and a hydrogen atom is shed, and the two shed hydrogen atoms are combined to generate hydrogen, and the broken primary carbon bond and the secondary carbon bond are combined to transform into a carbon-carbon double bond to generate propylene. Under the condition of 600° C., in a propane dehydrogenation reaction lasting up to 2000 minutes, the propane conversion rate is almost not reduced, and the conversion rate is reduced from 44.12% to 41%, and the catalyst has excellent stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a schematic diagram of the structure of the device used when the catalyst of the present invention is used;
[0027] In the figure, 1 is a propane gas cylinder, 2 is an argon gas cylinder, 3 is a hydrogen-argon gas cylinder, 4 is a first mass flow meter, 5 is a second mass flow meter, 6 is a third mass flow meter, 7 is a primary premixing device, 8 is a secondary premixing device, 9 is a temperature controller, 10 is a catalytic reactor, and 11 is a gas chromatograph;
[0028] Figure 2 This is a propane dehydrogenation reaction performance diagram of Comparative Examples 1-5 of the present invention, and the reaction conditions are: 600°C, 4mL / min high-purity propane + 36mL / min high-purity argon;
[0029] Figure 3 The propane dehydrogenation reaction performance diagram of Examples 1-3 and Comparative Example 3 of the present invention, the reaction conditions are 600°C, 4mL / min high-purity propane + 36mL / min hydrogen-argon gas (10% H2 + 90% Ar);
[0030] Figure 4 The XRD images of Examples 1-3 and Comparative Example 3 in the present invention are shown in FIG. DETAILED DESCRIPTION
[0031] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly and comprehensively understood.
[0032] First, the preparation method of the PtSn / Al2O3 catalyst in the present invention uses potassium chloroplatinite (K2PtCl4) and stannous chloride (SnCl2) as metal ion sources, tetrabutylammonium bromide (TBAB) as Pt coordination organic matter, dichloromethane (CH2Cl2) and tetrahydrofuran (THF) as metal organic solvents, and uses an electrostatic adsorption method to load PtSn-complex on Al2O3 to prepare Pt1Snx / Al2O3 catalyst.
[0033] First, the preparation method of PtSn / Al2O3 catalyst includes the following steps:
[0034] Prepare solution A: add 10.0-20.0 mg K2PtCl4 into 5.0-10.0 mL deionized water and shake evenly to obtain a light red, transparent and clear solution A;
[0035] Prepare solution B: add 10.0-30.0 mg of tetrabutylammonium bromide (TBAB) to 5.0-10.0 mL of dichloromethane (CH2Cl2), shake evenly to obtain a colorless, transparent, and clear uniform solution B;
[0036] Prepare solution C: Use a rubber-tipped dropper to transfer all of solution B to solution A. Shake vigorously and let stand until the solution is clearly separated. The supernatant is a colorless, transparent, and clear aqueous phase, and the lower supernatant is a light red, transparent, and clear organic solution. This process achieves the transfer of the Pt element from the aqueous phase to the organic phase. After removing the supernatant, a clear solution C is obtained;
[0037] Preparation of solution D: Dissolve 10.0-40.0 mg of stannous chloride (SnCl2) in 1-3 mL of tetrahydrofuran (THF), shake evenly and ultrasonicate for 20 min to completely dissolve the stannous chloride (SnCl2) to obtain solution D.
[0038] Preparation of solution E: At room temperature and 500 r / min, a certain amount of solution D was very slowly added to solution C, and the light red solution C was observed to gradually turn brownish red, and stirring was continued for 30 min to obtain solution E. The molar ratio of K2PtCl4 to SnCl2 was 1:1-5, preferably, the molar ratio of K2PtCl4 to SnCl2 was 1-5:1, preferably 1:1, 2:1, 3:1, 4:1 or 5:1.
[0039] Preparation of suspension F: Add 6 mL of tetrahydrofuran (THF) to 0.600 g of Al2O3, shake vigorously and ultrasonicate for 30 min to obtain Al2O3 suspension F.
[0040] The suspension F was immediately transferred to the solution E, and the stirring was continued at room temperature and 500r / min for 24h. After the stirring was completed, the liquid was removed after centrifugation at 8000r / min for 10min to obtain a light yellow solid product, which was vacuum dried at 60°C for 8-12h. After the drying was completed, the product was reduced at 500-600°C for 1-3h in an atmosphere of 40-80mL / min (10% H2 by volume + 90% Ar by volume), with a heating rate of 5-10°C / min. After the product was naturally cooled to room temperature, a PtSn / Al2O3 catalyst was obtained, which was recorded as Pt1Sn x / Al2O3 catalyst.
[0041] Pt1Sn of the present invention x / Al2O3 catalysts are metal clusters with a size of 1-2nm.
[0042] In the present invention, the theoretical loading amount of Pt is 1wt%. This method realizes the transfer of the active phase Pt from the aqueous phase to the organic phase, and adsorbs the active phase onto the carrier Al2O3 by electrostatic adsorption. In the present invention, the precursor of Pt is K2PtCl4, the precursor of Sn is SnCl2, the ligand is tetrabutylammonium bromide, and the organic solvent is dichloromethane and tetrahydrofuran. Only by using these raw materials can a special Pt-Sn characteristic coordination structure (Pt-Sn complex) be formed.
[0043] Pt1Sn in the present invention x / Application of Al2O3 in the field of propane dehydrogenation, the specific process is:
[0044] See also Figure 1 The test device used in the present invention includes a high-purity propane gas cylinder 1, a high-purity argon gas cylinder 2 and a high-purity hydrogen and argon gas cylinder 3. The outlet of the high-purity propane gas cylinder 1 is connected to the inlet of the first-stage premixing device 7 after passing through the first mass flowmeter 4, the outlet of the high-purity argon gas cylinder 2 is also connected to the inlet of the first-stage premixing device 7 after passing through the second mass flowmeter 5, the outlet of the high-purity hydrogen and argon gas cylinder 3 is connected to the inlet of the first-stage premixing device 7 after passing through the third mass flowmeter 6, the outlet of the first-stage premixing device 7 is connected to the inlet of the second-stage premixing device 8, the outlet of the second-stage premixing device 8 is connected to the inlet of the catalytic reactor 10, and the outlet of the catalytic reactor 10 is connected to the gas chromatograph 11. The catalytic reactor 10 includes a reaction tube, the outlet of the second-stage premixing device 8 is connected to the inlet of the reaction tube, and the outlet of the reaction tube is connected to the gas chromatograph 11. A thermal insulation layer is provided on the outer wall of the reaction tube. The first-stage premixing device 7, the second-stage premixing device 8 and the catalytic reactor 10 are all connected to a temperature controller 9.
[0045] The gas flow rate is strictly controlled by a mass flow meter: the propane flow rate is 4 mL / min and the argon flow rate is 36 mL / min. Propane and argon pass through the mass flow meter and enter the primary and secondary premixing devices at 120°C in turn, and are fully mixed and introduced into the catalytic reactor. The reaction process starts from room temperature and heats up to 600°C at a heating rate of 5°C / min. During the heating process, only high-purity argon is passed. When the temperature rises to 600°C, propane gas is introduced, and then the tail gas of the reaction device is passed into a gas chromatograph to detect its components.
[0046] When applied in the field of propane dehydrogenation, the reaction principle is: propane is adsorbed on the catalyst surface and combined with the activity, the primary carbon bond of propane breaks and a hydrogen atom is shed, then the secondary carbon bond breaks and a hydrogen atom is shed, the two hydrogen atoms shed combine to generate hydrogen, and the broken primary carbon bond and secondary carbon bond combine to transform into a carbon-carbon double bond to generate propylene.
[0047] In the present invention, after selecting the best PtSn ratio, the Zn element is used for modification, which greatly improves the stability of the catalyst.
[0048] First, the optimal PtSn ratio is screened in the present invention.
[0049] Comparative Example 1
[0050] Add 12.8 mg K2PtCl4 to 6.0 mL deionized water and shake evenly to obtain a light red, transparent and clear solution A;
[0051] Add 20.0 mg of tetrabutylammonium bromide (TBAB) into 6.0 mL of dichloromethane (CH2Cl2) and shake evenly to obtain a colorless, transparent, and clear uniform solution B;
[0052] Use a rubber-tipped dropper to transfer all of solution B into solution A. Shake vigorously and let stand until the solution is clearly separated into layers. The supernatant is a colorless, transparent, and clear aqueous phase, and the lower supernatant is a light red, transparent, and clear organic solution. After removing the supernatant, a clear lower supernatant C is obtained.
[0053] Dissolve 35.0 mg of stannous chloride (SnCl2) in 2 mL of tetrahydrofuran (THF), shake evenly and sonicate for 20 minutes to dissolve all the stannous chloride (SnCl2) to obtain solution D. At room temperature and 500 r / min, add 0.333 mL of solution D very slowly to solution C, and observe that the light red solution C gradually turns brownish red to obtain solution E, which is stirred for 30 minutes. The molar ratio of Pt to Sn is 1:1. Add 6 mL of tetrahydrofuran (THF) to 0.600 g of Al2O3, shake vigorously and sonicate for 30 minutes to obtain Al2O3 suspension F. Immediately transfer all of F to solution E, and continue stirring at room temperature and 500 r / min for 24 hours. After stirring, centrifuge at 8000 r / min for 10 minutes and remove the liquid to obtain a light yellow solid product, which is vacuum dried at 60°C for 12 hours. After drying, the catalyst was reduced at 600 °C for 2 h in an atmosphere of 60 mL / min (10% H2+90% Ar) with a heating rate of 5 °C / min. The catalyst was then naturally cooled to room temperature to obtain a Pt1Sn1 / Al2O3 catalyst.
[0054] Comparative Example 2
[0055] Add 12.8 mg K2PtCl4 to 6.0 mL deionized water and shake evenly to obtain a light red, transparent and clear solution A;
[0056] Add 20.0 mg of tetrabutylammonium bromide (TBAB) into 6.0 mL of dichloromethane (CH2Cl2) and shake evenly to obtain a colorless, transparent, and clear uniform solution B;
[0057] Use a rubber-tipped dropper to transfer all of solution B into solution A. Shake vigorously and let stand until the solution is clearly separated into layers. The supernatant is a colorless, transparent, and clear aqueous phase, and the lower supernatant is a light red, transparent, and clear organic solution. After removing the supernatant, a clear lower supernatant C is obtained.
[0058] Dissolve 35.0 mg of stannous chloride (SnCl2) in 2 mL of tetrahydrofuran (THF), shake evenly and sonicate for 20 minutes to dissolve all the stannous chloride (SnCl2) to obtain solution D. At room temperature and 500 r / min, add 0.667 mL of solution D to solution C very slowly, and observe that the light red solution C gradually turns brownish red to obtain solution E, which is stirred for 30 minutes. The molar ratio of Pt to Sn is 1:2. Add 6 mL of tetrahydrofuran (THF) to 0.600 g of Al2O3, shake vigorously and sonicate for 30 minutes to obtain Al2O3 suspension F. Immediately transfer all of F to solution E, and continue stirring at room temperature and 500 r / min for 24 hours. After stirring, centrifuge at 8000 r / min for 10 minutes and remove the liquid to obtain a light yellow solid product, which is vacuum dried at 60°C for 12 hours. After drying, the catalyst was reduced at 600 °C for 2 h in an atmosphere of 60 mL / min (10% H2 + 90% Ar) with a heating rate of 5 °C / min. The catalyst was then naturally cooled to room temperature to obtain a Pt1Sn2 / Al2O3 catalyst.
[0059] Comparative Example 3
[0060] Add 12.8 mg K2PtCl4 to 6.0 mL deionized water and shake evenly to obtain a light red, transparent and clear solution A;
[0061] Add 20.0 mg of tetrabutylammonium bromide (TBAB) into 6.0 mL of dichloromethane (CH2Cl2) and shake evenly to obtain a colorless, transparent, and clear uniform solution B;
[0062] Use a rubber-tipped dropper to transfer all of solution B into solution A. Shake vigorously and let stand until the solution is clearly separated into layers. The supernatant is a colorless, transparent, and clear aqueous phase, and the lower supernatant is a light red, transparent, and clear organic solution. After removing the supernatant, a clear lower supernatant C is obtained.
[0063] Dissolve 35.0 mg of stannous chloride (SnCl2) in 2 mL of tetrahydrofuran (THF), shake evenly and ultrasonicate for 20 minutes to dissolve all the stannous chloride (SnCl2) to obtain solution D. At room temperature and 500 r / min, add 1.000 mL of solution D very slowly to solution C, and observe that the light red solution C gradually turns brownish red to obtain solution E, which is stirred for 30 minutes. The molar ratio of Pt to Sn is 1:3. Add 6 mL of tetrahydrofuran (THF) to 0.600 g of Al2O3, shake vigorously and ultrasonicate for 30 minutes to obtain Al2O3 suspension F. Immediately transfer all of F to solution E, and continue stirring at room temperature and 500 r / min for 24 hours. After stirring, centrifuge at 8000 r / min for 10 minutes and remove the liquid to obtain a light yellow solid product, which is vacuum dried at 60°C for 12 hours. After drying, the catalyst was reduced at 600 °C for 2 h in an atmosphere of 60 mL / min (10% H2+90% Ar) with a heating rate of 5 °C / min. The catalyst was then naturally cooled to room temperature to obtain a Pt1Sn3 / Al2O3 catalyst.
[0064] Comparative Example 4
[0065] Add 12.8 mg K2PtCl4 to 6.0 mL deionized water and shake evenly to obtain a light red, transparent and clear solution A;
[0066] Add 20.0 mg of tetrabutylammonium bromide (TBAB) into 6.0 mL of dichloromethane (CH2Cl2) and shake evenly to obtain a colorless, transparent, and clear uniform solution B;
[0067] Use a rubber-tipped dropper to transfer all of solution B into solution A. Shake vigorously and let stand until the solution is clearly separated into layers. The supernatant is a colorless, transparent, and clear aqueous phase, and the lower supernatant is a light red, transparent, and clear organic solution. After removing the supernatant, a clear lower supernatant C is obtained.
[0068] Dissolve 35.0 mg of stannous chloride (SnCl2) in 2 mL of tetrahydrofuran (THF), shake evenly and sonicate for 20 minutes to dissolve all the stannous chloride (SnCl2) to obtain solution D. At room temperature and 500 r / min, add 1.333 mL of solution D very slowly to solution C, and observe that the light red solution C gradually turns brownish red to obtain solution E, which is stirred for 30 minutes. The molar ratio of Pt to Sn is 1:4. Add 6 mL of tetrahydrofuran (THF) to 0.600 g of Al2O3, shake vigorously and sonicate for 30 minutes to obtain Al2O3 suspension F. Immediately transfer all of F to solution E, and continue stirring at room temperature and 500 r / min for 24 hours. After stirring, centrifuge at 8000 r / min for 10 minutes and remove the liquid to obtain a light yellow solid product, which is vacuum dried at 60°C for 12 hours. After drying, the catalyst was reduced at 600 °C for 2 h in an atmosphere of 60 mL / min (10% H2+90% Ar) with a heating rate of 5 °C / min. The catalyst was then naturally cooled to room temperature to obtain a Pt1Sn4 / Al2O3 catalyst.
[0069] Comparative Example 5
[0070] Add 12.8 mg of K2PtCl4 to 6.0 mL of deionized water and shake evenly to obtain a light red, transparent and clear solution A;
[0071] Add 20.0 mg of tetrabutylammonium bromide (TBAB) into 6.0 mL of dichloromethane (CH2Cl2) and shake evenly to obtain a colorless, transparent, and clear uniform solution B;
[0072] Use a rubber-tipped dropper to transfer all of solution B into solution A. Shake vigorously and let stand until the solution is clearly separated into layers. The supernatant is a colorless, transparent, and clear aqueous phase, and the lower supernatant is a light red, transparent, and clear organic solution. After removing the supernatant, a clear lower supernatant C is obtained.
[0073] Dissolve 35.0 mg of stannous chloride (SnCl2) in 2 mL of tetrahydrofuran (THF), shake evenly and sonicate for 20 minutes to dissolve all the stannous chloride (SnCl2) to obtain solution D. At room temperature and 500 r / min, add 1.667 mL of solution D very slowly to solution C, and observe that the light red solution C gradually turns brownish red to obtain solution E, which is stirred for 30 minutes. The molar ratio of Pt to Sn is 1:5. Add 6 mL of tetrahydrofuran (THF) to 0.600 g of Al2O3, shake vigorously and sonicate for 30 minutes to obtain Al2O3 suspension F. Immediately transfer all of F to solution E, and continue stirring at room temperature and 500 r / min for 24 hours. After stirring, centrifuge at 8000 r / min for 10 minutes and remove the liquid to obtain a light yellow solid product, which is vacuum dried at 60°C for 12 hours. After drying, the catalyst was reduced at 600 °C for 2 h in an atmosphere of 60 mL / min (10% H2+90% Ar) with a heating rate of 5 °C / min. The catalyst was then naturally cooled to room temperature to obtain a Pt1Sn5 / Al2O3 catalyst.
[0074] Pt1Sn x / Al2O3 was used for propane dehydrogenation reaction, and the best performance sample Pt1Sn3 / Al2O3 was screened out, such as Figure 2 As shown, it can be seen that Pt1Sn3 / Al2O3 has the best propane conversion, with an initial activity close to 60%. The catalyst performance drops from 60% to 30% within 20 h, during which the selectivity of propylene exceeds 99.9%.
[0075] Example 1
[0076] Prepare solution A: Add 12.8 mg K2PtCl4 into 6.0 mL deionized water and shake evenly to obtain a light red, transparent and clear solution A.
[0077] Prepare solution B: add 4.2 mg of ZnCl2 into 200 μL of 0.1 mol / L hydrochloric acid and shake evenly to obtain a colorless, transparent and homogeneous solution B;
[0078] Take a certain amount of solution B and add it to solution A. Shake thoroughly to obtain a light red, transparent and clear solution C. The amount of solution B is 20 μL.
[0079] Prepare solution D: Add 20.0 mg of tetrabutylammonium bromide (TBAB) to 6.0 mL of dichloromethane (CH2Cl2) and shake evenly to obtain a colorless, transparent, and clear uniform solution D;
[0080] Prepare solution E: Use a rubber-tipped dropper to transfer all of solution D to solution C. Shake vigorously and let stand until the solution is clearly separated. The supernatant is a colorless, transparent, and clear aqueous phase, and the lower supernatant is a light red, transparent, and clear organic solution. This process achieves the transfer of the Pt element from the aqueous phase to the organic phase. After removing the supernatant, a clear lower supernatant is obtained to obtain solution E;
[0081] Prepare solution F: Dissolve stannous chloride (SnCl2) in 1 mL of tetrahydrofuran (THF), shake evenly, and ultrasonicate for 20 minutes to completely dissolve the stannous chloride (SnCl2).
[0082] At room temperature and 500 r / min, solution F was added to solution E very slowly. The light red solution E was observed to gradually turn brownish red to obtain solution G. Stirring was continued for 30 min. The molar ratio of Pt, Zn, and Sn was 1:0.1:3;
[0083] Preparation of suspension H: Add 6 mL of tetrahydrofuran (THF) to 0.600 g of Al2O3, shake vigorously and ultrasonicate for 30 min to obtain Al2O3 suspension H.
[0084] The suspension H was immediately transferred to the solution G and stirred for 24 hours at room temperature and 500 r / min. After stirring, the suspension was centrifuged at 8000 r / min for 10 minutes and the liquid was removed to obtain a light yellow solid product, which was vacuum dried at 60°C for 12 hours. After drying, the suspension was reduced at 600°C for 2 hours in an atmosphere of 60 mL / min (10% H2+90% Ar) at a heating rate of 5°C / min. After cooling naturally to room temperature, the catalyst, Pt1Zn 0.1 Sn3 / Al2O3 catalyst.
[0085] Example 2
[0086] Prepare solution A: Add 12.8 mg K2PtCl4 into 6.0 mL deionized water and shake evenly to obtain a light red, transparent and clear solution A.
[0087] Prepare solution B: add 4.2 mg of ZnCl2 into 200 μL of 0.1 mol / L hydrochloric acid and shake evenly to obtain a colorless, transparent and homogeneous solution B;
[0088] Take a certain amount of solution B and add it to solution A. Shake thoroughly to obtain a light red, transparent and clear solution C. The amount of solution B is 100 μL.
[0089] Prepare solution D: Add 20.0 mg of tetrabutylammonium bromide (TBAB) to 6.0 mL of dichloromethane (CH2Cl2) and shake evenly to obtain a colorless, transparent, and clear uniform solution D;
[0090] Use a rubber-tipped dropper to transfer all of solution D to solution C. Shake vigorously and let stand until the solution is clearly separated. The supernatant is a colorless, transparent, and clear aqueous phase, and the lower supernatant is a light red, transparent, and clear organic solution. This process achieves the transfer of the Pt element from the aqueous phase to the organic phase. After removing the supernatant, a clear lower supernatant E is obtained;
[0091] Prepare solution F: Dissolve 17.5 mg of stannous chloride (SnCl2) in 1 mL of tetrahydrofuran (THF), shake evenly, and sonicate for 20 minutes to completely dissolve the stannous chloride (SnCl2).
[0092] At room temperature and 500 r / min, solution F was added to solution E very slowly. The light red solution E was observed to gradually turn brownish red to obtain solution G. Stirring was continued for 30 min. The molar ratio of Pt, Zn, and Sn was 1:0.5:3;
[0093] Preparation of suspension H: Add 6 mL of tetrahydrofuran (THF) to 0.600 g of Al2O3, shake vigorously and ultrasonicate for 30 min to obtain Al2O3 suspension H. Immediately transfer all of suspension H to solution G, and continue stirring at room temperature and 500 r / min for 24 h. After stirring, centrifuge at 8000 r / min for 10 min to remove the liquid to obtain a light yellow solid product, which was vacuum dried at 60°C for 12 h. After drying, reduce at 600°C for 2 h in an atmosphere of 60 mL / min (10% H2 + 90% Ar), with a heating rate of 5°C / min, and cool naturally to room temperature to obtain the catalyst, namely Pt1Zn 0.5 Sn3 / Al2O3 catalyst.
[0094] Example 3
[0095] Prepare solution A: Add 12.8 mg K2PtCl4 into 6.0 mL deionized water and shake evenly to obtain a light red, transparent and clear solution A.
[0096] Prepare solution B: add 4.2 mg of ZnCl2 into 200 μL of 0.1 mol / L hydrochloric acid and shake evenly to obtain a colorless, transparent and homogeneous solution B;
[0097] Take a certain amount of solution B and add it to solution A. Shake thoroughly to obtain a light red, transparent and clear solution C. The amount of solution B is 140 μL.
[0098] Prepare solution D: Add 20.0 mg of tetrabutylammonium bromide (TBAB) to 6.0 mL of dichloromethane (CH2Cl2) and shake evenly to obtain a colorless, transparent, and clear uniform solution D;
[0099] Use a rubber-tipped dropper to transfer all of solution D to solution C. Shake vigorously and let stand until the solution is clearly separated. The supernatant is a colorless, transparent, and clear aqueous phase, and the lower supernatant is a light red, transparent, and clear organic solution. This process achieves the transfer of the Pt element from the aqueous phase to the organic phase. After removing the supernatant, a clear lower supernatant E is obtained;
[0100] Prepare solution F: Dissolve 17.5 mg of stannous chloride (SnCl2) in 1 mL of tetrahydrofuran (THF), shake evenly, and sonicate for 20 minutes to completely dissolve the stannous chloride (SnCl2).
[0101] At room temperature and 500 r / min, solution F was added to solution E very slowly. The light red solution E was observed to gradually turn brownish red to obtain solution G. Stirring was continued for 30 min. The molar ratio of Pt, Zn, and Sn was 1:0.7:3;
[0102] Preparation of suspension H: Add 6 mL of tetrahydrofuran (THF) to 0.600 g of Al2O3, shake vigorously and ultrasonicate for 30 min to obtain Al2O3 suspension H. Immediately transfer all of suspension H to solution G, and continue stirring at room temperature and 500 r / min for 24 h. After stirring, centrifuge at 8000 r / min for 10 min to remove the liquid to obtain a light yellow solid product, which was vacuum dried at 60°C for 12 h. After drying, reduce at 600°C for 2 h in an atmosphere of 60 mL / min (10% H2 + 90% Ar), with a heating rate of 5°C / min, and cool naturally to room temperature to obtain the catalyst, namely Pt1Zn 0.7 Sn3 / Al2O3 catalyst.
[0103] Pt1Zn x Sn3 / Al2O3 was used for propane dehydrogenation reaction, and the best performance sample Pt1Zn was screened out 0.5 Sn3 / Al2O3.
[0104] See also Figure 3 The amount of Zn doping has different effects on the propane dehydrogenation performance of the samples. The conversion rate of Pt1Sn3 / Al2O3 without Zn doping (Comparative Example 3) decreased from 45% to 34.6% within 500min, and the propane conversion rate decreased at a rate of 0.0208% / min. Compared with Pt1Sn3 / Al2O3, Pt1Zn3 / Al2O3 with a small amount of Zn doping 0.1 Sn3 / Al2O3 (Example 1) and Excess Zn Doped Pt1Zn 0.7The activity and stability of Sn3 / Al2O3 (Example 3) decreased to varying degrees, from 34% and 34.2% to 22.24% and 25.53% respectively within 500 min, and the propane conversion rate decreased at 0.0235% / min and 0.01734% / min respectively; while the Pt1Zn doped with appropriate amount of Zn 0.5 Sn3 / Al2O3 (Example 2) has a very significant improvement in stability. Within 2000 min, the propane conversion rate hardly decreased, from 44.12% to 41%, and the propane conversion rate decreased at a rate of only 0.00156% / min, which greatly improved the stability of the catalyst. x The Sn3 / Al2O3 samples all showed over 99% propylene selectivity during the PDH reaction.
[0105] See also Figure 4 All samples of Examples 1-3 showed characteristic peaks that were exactly the same as those of the carrier Al2O3, indicating that the active phase was evenly distributed on the carrier.
[0106] The catalyst prepared by the invention has high activity, stability and ultra-high propylene selectivity, and the preparation process is simple and the raw material price is low.
[0107] Example 4
[0108] Based on the Pt1Sn3 / Al2O3 in Comparative Example 3, Zn element is doped for modification to further improve the performance of the catalyst. The specific preparation process includes the following steps:
[0109] First, prepare solution A: add K2PtCl4 into deionized water and shake evenly to obtain a light red, transparent and clear solution A;
[0110] Prepare solution B: Add ZnCl2 to 0.1 mol / L hydrochloric acid and shake evenly to obtain a colorless, transparent and clear uniform solution B;
[0111] Take a certain amount of solution B and add it to solution A. Shake it thoroughly to obtain a light red, transparent and clear solution C.
[0112] Prepare solution D: Add tetrabutylammonium bromide (TBAB) into dichloromethane (CH2Cl2) and shake evenly to obtain a colorless, transparent and clear uniform solution D;
[0113] Use a rubber-tipped dropper to transfer all of solution D to solution C. After vigorous shaking, let it stand until the solution is clearly separated. The supernatant is a colorless, transparent, and clear aqueous phase, and the lower supernatant is a light red, transparent, and clear organic solution. This process achieves the transfer of the Pt element from the aqueous phase to the organic phase. After removing the supernatant, a clear lower supernatant is obtained to obtain solution E;
[0114] Prepare solution F: Dissolve stannous chloride (SnCl2) in tetrahydrofuran (THF), shake evenly and sonicate for 20 minutes to completely dissolve the stannous chloride (SnCl2).
[0115] At room temperature and 500 r / min, solution F was added to solution E very slowly. The light red solution E was observed to gradually turn brownish red to obtain solution G. Stirring was continued for 30 min. The molar ratio of zinc chloride, K2PtCl4 and stannous chloride was 0.1:1:2; the mass ratio of tetrabutylammonium bromide and potassium chloroplatinite was 1:1;
[0116] Preparation of suspension H: Add tetrahydrofuran (THF) to Al2O3, shake vigorously and ultrasonicate for 30 minutes to obtain Al2O3 suspension H. Immediately transfer all of suspension H to solution G, and continue stirring at room temperature and 500r / min for 24 hours. After stirring, centrifuge at 8000r / min for 10 minutes to remove the liquid to obtain a light yellow solid product, which was vacuum dried at 60°C for 12 hours. After drying, reduce at 500°C for 2 hours in an atmosphere of 60mL / min (10% H2+90% Ar), with a heating rate of 10°C / min, and cool naturally to room temperature to obtain Pt1Zn x Sn3 / Al2O3 catalyst, wherein the mass ratio of Al2O3 to potassium chloroplatinite is 0.600:10.0.
[0117] Example 5
[0118] First, prepare solution A: add K2PtCl4 into deionized water and shake evenly to obtain a light red, transparent and clear solution A;
[0119] Prepare solution B: Add ZnCl2 to 0.1 mol / L hydrochloric acid and shake evenly to obtain a colorless, transparent and clear uniform solution B;
[0120] Take a certain amount of solution B and add it to solution A. Shake it thoroughly to obtain a light red, transparent and clear solution C.
[0121] Prepare solution D: Add tetrabutylammonium bromide (TBAB) into dichloromethane (CH2Cl2) and shake evenly to obtain a colorless, transparent and clear uniform solution D;
[0122] Use a rubber-tipped dropper to transfer all of solution D to solution C. After vigorous shaking, let it stand until the solution is clearly separated. The supernatant is a colorless, transparent, and clear aqueous phase, and the lower supernatant is a light red, transparent, and clear organic solution. This process achieves the transfer of the Pt element from the aqueous phase to the organic phase. After removing the supernatant, a clear lower supernatant is obtained to obtain solution E;
[0123] Prepare solution F: Dissolve stannous chloride (SnCl2) in tetrahydrofuran (THF), shake evenly and sonicate for 20 minutes to completely dissolve the stannous chloride (SnCl2).
[0124] At room temperature and 500 r / min, solution F was added to solution E very slowly. The light red solution E was observed to gradually turn brownish red to obtain solution G. Stirring was continued for 30 min. The molar ratio of zinc chloride, K2PtCl4 and stannous chloride was 0.3:1:3; the mass ratio of tetrabutylammonium bromide and potassium chloroplatinite was 1:2;
[0125] Preparation of suspension H: Add tetrahydrofuran (THF) to Al2O3, shake vigorously and ultrasonicate for 30 minutes to obtain Al2O3 suspension H. Immediately transfer all of suspension H to solution G, and continue stirring at room temperature and 500r / min for 24 hours. After stirring, centrifuge at 8000r / min for 10 minutes and remove the liquid to obtain a light yellow solid product, which is vacuum dried at 60°C for 12 hours. After drying, reduce at 550°C for 2 hours in an atmosphere of 60mL / min (10% H2+90% Ar), with a heating rate of 7°C / min, and cool naturally to room temperature to obtain Pt1Zn x Sn3 / Al2O3 catalyst, wherein the mass ratio of Al2O3 to potassium chloroplatinite is 0.600:20.0.
[0126] Example 6
[0127] First, prepare solution A: add K2PtCl4 into deionized water and shake evenly to obtain a light red, transparent and clear solution A;
[0128] Prepare solution B: Add ZnCl2 to 0.1 mol / L hydrochloric acid and shake evenly to obtain a colorless, transparent and clear uniform solution B;
[0129] Take a certain amount of solution B and add it to solution A. Shake it thoroughly to obtain a light red, transparent and clear solution C.
[0130] Prepare solution D: Add tetrabutylammonium bromide (TBAB) into dichloromethane (CH2Cl2) and shake evenly to obtain a colorless, transparent and clear uniform solution D;
[0131] Use a rubber-tipped dropper to transfer all of solution D to solution C. After vigorous shaking, let it stand until the solution is clearly separated. The supernatant is a colorless, transparent, and clear aqueous phase, and the lower supernatant is a light red, transparent, and clear organic solution. This process achieves the transfer of the Pt element from the aqueous phase to the organic phase. After removing the supernatant, a clear lower supernatant is obtained to obtain solution E;
[0132] Prepare solution F: Dissolve stannous chloride (SnCl2) in tetrahydrofuran (THF), shake evenly and sonicate for 20 minutes to completely dissolve the stannous chloride (SnCl2).
[0133] At room temperature and 500 r / min, solution F was added to solution E very slowly. The light red solution E was observed to gradually turn brownish red to obtain solution G. Stirring was continued for 30 min. The molar ratio of zinc chloride, K2PtCl4 and stannous chloride was 0.5:1:1; the mass ratio of tetrabutylammonium bromide and potassium chloroplatinite was 3:1;
[0134] Preparation of suspension H: Add tetrahydrofuran (THF) to Al2O3, shake vigorously and ultrasonicate for 30 minutes to obtain Al2O3 suspension H. Immediately transfer all of suspension H to solution G, and continue stirring at room temperature and 500r / min for 24 hours. After stirring, centrifuge at 8000r / min for 10 minutes and remove the liquid to obtain a light yellow solid product, which is vacuum dried at 60°C for 12 hours. After drying, reduce at 570°C for 2 hours in an atmosphere of 60mL / min (10% H2+90% Ar), with a heating rate of 6°C / min, and cool naturally to room temperature to obtain Pt1Zn x Sn3 / Al2O3 catalyst, wherein the mass ratio of Al2O3 to potassium chloroplatinite is 0.600:13.
[0135] Example 7
[0136] First, prepare solution A: add K2PtCl4 into deionized water and shake evenly to obtain a light red, transparent and clear solution A;
[0137] Prepare solution B: Add ZnCl2 to 0.1 mol / L hydrochloric acid and shake evenly to obtain a colorless, transparent and clear uniform solution B;
[0138] Take a certain amount of solution B and add it to solution A. Shake it thoroughly to obtain a light red, transparent and clear solution C.
[0139] Prepare solution D: Add tetrabutylammonium bromide (TBAB) into dichloromethane (CH2Cl2) and shake evenly to obtain a colorless, transparent and clear uniform solution D;
[0140] Use a rubber-tipped dropper to transfer all of solution D to solution C. After vigorous shaking, let it stand until the solution is clearly separated. The supernatant is a colorless, transparent, and clear aqueous phase, and the lower supernatant is a light red, transparent, and clear organic solution. This process achieves the transfer of the Pt element from the aqueous phase to the organic phase. After removing the supernatant, a clear lower supernatant is obtained to obtain solution E;
[0141] Prepare solution F: Dissolve stannous chloride (SnCl2) in tetrahydrofuran (THF), shake evenly and sonicate for 20 minutes to completely dissolve the stannous chloride (SnCl2).
[0142] At room temperature and 500 r / min, solution F was added to solution E very slowly. It was observed that the light red solution E gradually turned brownish red to obtain solution G, and stirring was continued for 30 min. The molar ratio of zinc chloride, K2PtCl4 and stannous chloride was 0.7:1:5; the mass ratio of tetrabutylammonium bromide and potassium chloroplatinite was 3:2;
[0143] Preparation of suspension H: Add tetrahydrofuran (THF) to Al2O3, shake vigorously and ultrasonicate for 30 minutes to obtain Al2O3 suspension H. Immediately transfer all of suspension H to solution G, and continue stirring at room temperature and 500r / min for 24 hours. After stirring, centrifuge at 8000r / min for 10 minutes and remove the liquid to obtain a light yellow solid product, which is vacuum dried at 60°C for 12 hours. After drying, reduce at 600°C for 2 hours in an atmosphere of 60mL / min (10% H2+90% Ar), with a heating rate of 5°C / min, and cool naturally to room temperature to obtain Pt1Zn x Sn3 / Al2O3 catalyst, wherein the mass ratio of Al2O3 to potassium chloroplatinite is 0.600:17.
[0144] The present invention is in Pt1Sn x / Al2O3 is modified to further improve the performance. When x=3, the performance of the catalyst is the best. x / Al2O3 is doped with Zn element. An appropriate amount of Zn has a positive effect on the catalyst, while a small amount or an excess of Zn will produce side effects on the catalyst.
[0145] The above description is only for the best embodiment of the present invention, but it should not be understood as limiting the claims. The present invention is not limited to the above embodiments, and its specific structure is allowed to be changed. However, all changes made within the protection scope of the independent claims of the present invention are within the protection scope of the present invention.
[0146] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
Claims
1. A method for preparing a Zn-regulated PtSn / Al2O3 catalyst, characterized in that: A metal ion source containing platinum and tin and a Pt-coordinated organic matter are placed in an organic solvent and an electrostatic adsorption method is used to prepare a Zn-regulated PtSn / Al2O3 catalyst; the metal ion source containing platinum and tin includes potassium chloroplatinite and stannous chloride.
2. The method for preparing the Zn-regulated PtSn / Al2O3 catalyst according to claim 1, characterized in that: The following steps are involved: Adding the acid solution of zinc chloride to the potassium chloroplatinite solution, then adding the dichloromethane solution of the Pt coordinated organic matter, separating the layers, and taking the lower layer to obtain a clear solution; Adding the tetrahydrofuran solution of stannous chloride to the clear solution, stirring evenly, to obtain a mixed solution; Adding a suspension of aluminum oxide in tetrahydrofuran to the mixed solution, stirring to obtain a solid; The solid is dried and calcined to obtain a Zn-regulated PtSn / Al2O3 catalyst.
3. The method for preparing the Zn-regulated PtSn / Al2O3 catalyst according to claim 2, characterized in that: The molar ratio of zinc chloride, potassium chloroplatinite and stannous chloride is (0.1-0.7):1:(1-5).
4. The method for preparing the Zn-regulated PtSn / Al2O3 catalyst according to claim 1 or 2, characterized in that: The Pt coordinated organic compound is tetrabutylammonium bromide.
5. According to the preparation method of the Zn-regulated PtSn / Al2O3 catalyst according to claim 1 or 2, the mass ratio of the Pt-coordinated organic matter to potassium chloroplatinite is 10.0-30.0:10.0-20.
0.
6. The method for preparing the Zn-regulated PtSn / Al2O3 catalyst according to claim 2, characterized in that: The mass ratio of aluminum oxide to potassium chloroplatinite is 0.600:10.0-20.
0.
7. The method for preparing the Zn-regulated PtSn / Al2O3 catalyst according to claim 2, characterized in that: The calcination temperature is 500-600°C and the calcination time is 1-3h.
8. The method for preparing the Zn-regulated PtSn / Al2O3 catalyst according to claim 7, characterized in that: The calcination is carried out under a mixture of H2 and Ar; the temperature is increased to 500-600°C at a heating rate of 5-10°C / min.
9. A Zn-regulated PtSn / Al2O3 catalyst prepared according to the method of claim 1 or 2, characterized in that: The catalyst is a metal cluster with a size of 1-2 nm.
10. Use of a Zn-regulated PtSn / Al2O3 catalyst prepared according to the method of claim 1 or 2 in propane dehydrogenation.
Citation Information
Patent Citations
Supported platinum based three-way catalyst and preparing method and use
CN101164690A
Method for preparing low-carbon alkane dehydrogenation catalyst
CN105521779A
Preparation method of low-carbon alkane dehydrogenation catalyst
CN108786798A
Low-carbon alkane dehydrogenation method
CN114621047A
Cited By
Iron-based molecular sieve catalyst, preparation method and application thereof
CN120502359A