Hydrothermally stable core-shell structure three-way catalyst and preparation method and application thereof
By loading a hydrothermal and stable three-effect catalyst with a low-content precious metal core-shell structure on the support material, the problems of easy agglomeration of catalysts at high temperatures and high loads of precious metals in the prior art are solved, and efficient natural gas exhaust purification is achieved, reducing the reduction of natural gas emissions cost and energy consumption.
Patent Information
- Application Number
- CN202410629728.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-21
- Publication Date
- 2024-11-22
AI Technical Summary
The existing three-effect catalysts are prone to agglomeration at high temperatures and high loading of precious metals lead to increased costs and energy consumption, and lack of thermal stability, making it difficult to meet the strict requirements for natural gas exhaust purification.
The three-effect catalyst for stable core-shell structures is adopted to load the low-content precious metal core-shell structure on the support material, and use precious metals such as Pd, Rh, and Pt and shell materials such as zirconia and ceria to combine electrostatic gravity and supramolecular Self-assembly method to prepare to form an efficient catalyst.
It significantly improves the thermal stability and activity of the catalyst, extends the service life, reduces the load of precious metals, reduces production costs, is suitable for high-temperature exhaust gas purification, and is especially suitable for exhaust gas treatment of compressed natural gas engines.
Smart Images

Figure CN118988303A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of automobile exhaust catalysts, and specifically relates to a three-way catalyst for natural gas vehicles, namely, a hydrothermally stable core-shell structure three-way catalyst and a preparation method and application thereof. Background Art
[0002] With the development of social economy and the continuous improvement of people's living standards, the number of cars in my country continues to increase, and the problem of urban air pollution is becoming increasingly serious. In response to this challenge, my country has put forward more stringent standards and requirements for the control of motor vehicle exhaust emissions. At present, three-way catalytic technology (TWC) has become the mainstream technology for heavy-duty natural gas engine exhaust treatment. Through the three-way catalyst, the main pollutants emitted by motor vehicles (such as CH4, CO and NO x ) can be effectively converted into harmless substances such as carbon dioxide, nitrogen and water. However, since it is more difficult to purify CH4 in the exhaust gas of natural gas vehicles than HC in traditional gasoline vehicles, a catalyst with higher activity is required.
[0003] Currently, the active components used in three-way catalysts are mainly based on precious metals, such as palladium, rhodium, platinum, etc., but these materials tend to agglomerate at high temperatures, resulting in reduced catalytic activity and increased costs. In addition, faced with the reduction of precious metal resources and increasingly stringent emission regulations, the current three-way catalyst industry urgently needs to reduce the precious metal content while improving the activity and thermal stability of the catalyst.
[0004] Traditional three-way catalysts usually use precious metal salts loaded on a carrier with good thermal stability to form catalytically active precious metal nanoparticles. However, this type of catalyst has several problems: first, the high precious metal loading leads to high cost and high energy consumption; second, the precious metals are not resistant to high temperatures and are prone to agglomeration or shedding at high temperatures, thereby reducing the service life and activity of the catalyst. Summary of the invention
[0005] In view of the above-mentioned deficiencies in the prior art, the present application provides a high-efficiency hydrothermally stable core-shell three-way catalyst that can significantly improve catalyst performance and service life while reducing precious metal loading and production costs.
[0006] In order to solve the above technical problems, the technical solution adopted in the present application is: a high-efficiency hydrothermally stable core-shell structure three-way catalyst, which is composed of a core-shell structure containing active components and a carrier material, and the core-shell structure is loaded into the carrier material; the core component in the core-shell structure is a precious metal, and its content is 0.1-5wt% of the total weight of the catalyst; the shell component in the core-shell structure is a solid solution or a combination thereof, and its content is 10-60wt% of the total weight of the catalyst, and the balance is the carrier material.
[0007] Furthermore, the noble metal is one or a combination of noble metals such as Pd, Rh, Pt, Au, etc.
[0008] Furthermore, the noble metal is Pd.
[0009] Furthermore, the content of the noble metal is 0.5-2wt% based on the total weight of the catalyst.
[0010] Furthermore, the shell component is selected from zirconium oxide, ceria, a solid solution of cerium and zirconium, or a combination thereof.
[0011] Furthermore, the shell component is cerium dioxide.
[0012] Furthermore, the content of cerium dioxide (CeO2) is 10wt% to 40wt% of the total amount of the catalyst, and the content of zirconium oxide (ZrO2) is 10 to 20wt% of the total amount of the catalyst (the two can be added either alone or simultaneously).
[0013] Furthermore, the carrier material includes one or a combination of oxygen storage materials and / or alumina (Al2O3) or cerium aluminum solid solution.
[0014] Furthermore, the carrier material may be doped with structural additives such as BaO, La2O3 or Y2O3, with a content of 3-10wt% of the total amount of the catalyst.
[0015] Furthermore, the carrier material is alumina.
[0016] Furthermore, the catalyst loading method includes electrostatic attraction and supramolecular self-assembly method.
[0017] The present application also provides a method for preparing the above-mentioned efficient hydrothermally stable core-shell structure three-way catalyst, the preparation steps comprising:
[0018] (1) Synthesis of core-shell structured nanoparticles: A noble metal precursor and a shell material precursor are added by an inorganic salt-assisted self-oxidation-reduction method, and then ammonia water is added, followed by heating, centrifugal washing and drying to obtain core-shell structured nanoparticles;
[0019] (2) Preparation and surface modification of the carrier: the carrier powder is dispersed in ammonia water and heated to improve the surface properties of the carrier; or the carrier powder is mixed with octyltrimethoxysilane (TEOOS), and then refluxed, centrifuged and dried to obtain a hydrophobic carrier;
[0020] (3) Core-shell structure supported catalyst: the carrier powder of step (2) is dispersed and heated in an aqueous solution containing ammonia or a tetrahydrofuran solution, and then the core-shell structure nanoparticles are added to the reaction system and continue to be heated, and finally centrifugally dried to obtain a catalyst powder;
[0021] (4) Heat treatment: The catalyst powder obtained in step (3) is calcined for 3-6 hours to obtain a three-way catalyst.
[0022] Furthermore, the inorganic salt in step (1) is at least one of KBr, KCl and KI.
[0023] Furthermore, the noble metal precursor described in step (1) includes one or more of sodium tetrachloropalladate, potassium chloroplatinite, and rhodium trichloride trihydrate.
[0024] Furthermore, the noble metal precursor in step (1) is sodium tetrachloropalladate.
[0025] Furthermore, the shell material precursor described in step (1) is a soluble salt solution of one or more of cerium nitrate hexahydrate, cerium acetate, and zirconium nitrate.
[0026] Furthermore, the shell material precursor in step (1) is cerium nitrate hexahydrate.
[0027] Furthermore, the core-shell structure nanoparticles described in step (1) also include oleic acid modification thereof, specifically: after the ammonia water is added dropwise, an oleic acid solution mixed in CHCl3 is added to the reaction system for modification.
[0028] Furthermore, when the core-shell structured nanoparticles described in step (4) are oleic acid-modified core-shell structured nanoparticles, the hydrophobic carrier is dispersed in a tetrahydrofuran solution.
[0029] Furthermore, the carrier powder in step (2) is a mixture of an oxygen storage material and alumina or a combination of one or more of a cerium-aluminum solid solution.
[0030] Furthermore, the carrier powder in step (2) is γ-phase activated alumina.
[0031] Furthermore, the loading method of the core-shell structure-loaded catalyst in step (3) includes electrostatic attraction and supramolecular self-assembly method.
[0032] Furthermore, the calcination conditions described in step (4) are a muffle furnace heating rate of 3°C / min, and a calcination temperature set to 500°C or 850°C.
[0033] The present application also provides specific applications of the above-mentioned catalyst, which is suitable for treating harmful gases in high-temperature exhaust gas, and is particularly suitable for exhaust gas purification of compressed natural gas (CNG) engines. It can effectively convert exhaust gas components such as CH4, CO, NO, etc., while maintaining high hydrothermal stability and long-term durability.
[0034] Compared with the prior art, this application has the following significant advantages and outstanding merits:
[0035] 1 Enhanced thermal stability and hydrothermal stability: The catalyst of the present application utilizes its unique core-shell structure design to significantly improve its stability in extremely high temperature and water vapor environments; compared with the problem of traditional catalysts being easily agglomerated and deactivated at high temperatures, the catalyst of the present application can maintain its high-efficiency catalytic performance in a wider temperature range (100-750°C), thereby extending its service life and reducing the frequency of replacement, effectively reducing the total cost of long-term operation.
[0036] 2. Improve catalytic activity: This application precisely controls the material composition, structural layout and content of the core and shell to make the catalyst exhibit excellent catalytic activity in the process of natural gas vehicle exhaust purification; especially in the conversion of CH4, CO and NO x In terms of pollutants, even under low temperature conditions ("low temperature" usually refers to the operating range where the catalyst begins to show activity but has not yet reached the optimal performance level, low temperature conditions usually refer to the range of about 200°C to 350°C) and high temperature conditions (high temperature conditions have a rough temperature range of 600-800°C. The core-shell structure catalyst has good thermal stability and is tested in a relatively wide temperature range and maintains high catalytic performance (100-750°C range). The maximum test temperature of most existing catalysts only reaches 500°C, but the actual exhaust emission temperature will reach 600-800°C high temperature conditions), it can maintain high efficiency performance, effectively reduce exhaust emissions, and make important contributions to environmental protection.
[0037] 3. Reduce the loading of precious metals: Through the innovative preparation method and unique core-shell structure proposed in this application, the use of precious metals can be significantly reduced while maintaining the high performance of the catalyst; this not only reduces the direct production cost of the catalyst, but also reduces the dependence on precious metal resources, increases the market competitiveness of the catalyst, and makes it more suitable for large-scale industrial production and wide application.
[0038] 4. Simplified preparation process: This application simplifies the catalyst preparation process through self-oxidation-reduction one-step synthesis and self-assembly technology assisted by salting-out effect; compared with the traditional complex and high-energy consumption preparation method, this method improves production efficiency, reduces energy consumption and production costs, and has significant industrial application value and broad market prospects; in summary, this application provides a significantly improved high-efficiency hydrothermal stable three-way catalyst for natural gas vehicle exhaust purification technology through innovative core-shell structure design and efficient preparation method. These advantages indicate that this application has important application potential and commercial value in the field of environmental protection.
[0039] 5. The core-shell structure of the catalyst of the present application has broad application prospects in improving the thermal stability, activity and durability of the catalyst due to its unique structural advantages; the catalyst is precisely constructed from three basic components: a central metal core, such as palladium (Pd) or platinum (Pt), which provides the core's catalytic activity; an outer stabilizing shell material, such as cerium dioxide (CeO2) or zirconium dioxide ZrO2, which protects the metal core to enhance the overall stability; and finally the core-shell structure is loaded on a carrier material, such as alumina (Al2O3), to form a complete core-shell structure catalyst system; this unique three-layer structure not only promotes the synergistic effect between the core and the shell, further improving the catalytic efficiency and stability, but also ensures the efficient application and long-term stability of the catalyst by loading it on a suitable carrier; at the same time, the structure has high design flexibility and can be optimized according to specific conditions of use, perfectly meeting the needs of the field of natural gas vehicle exhaust treatment.
[0040] 6. The catalyst of the present application may also be added with structural additives, such as BaO, La2O3 or Y2O3 of the present application, which may be added in addition to the main components such as oxygen storage materials or alumina (Al2O3) or cerium aluminum solid solution; the addition of structural additives to the catalyst not only improves the thermal stability and sintering resistance of the catalyst, but also enhances the activity and selectivity of the catalyst in complex chemical reactions; these additives optimize the function of the catalyst by changing the properties of the catalyst surface and improving the distribution of the internal structure; for example: BaO: increases the alkalinity of the catalyst, helps to absorb and neutralize acidic gases, thereby improving the NO xreduction efficiency; La2O3: enhances the structural stability of the catalyst, provides more redox active sites, thereby increasing the oxygen storage capacity and release capacity of the catalyst, which is particularly beneficial to improving the conversion efficiency of CO and HC; Y2O3: improves the thermal stability of the catalyst, which helps to maintain the activity and structure of the catalyst without being destroyed in a high temperature environment; through the synergistic effect of these additives, the catalyst can maintain high efficiency in a wider temperature range and has a stronger adaptability to environmental conditions, especially in applications such as automobile exhaust purification that require long-term stable operation. This improvement is particularly important; these optimization measures enable the catalyst to not only start quickly at low temperatures, but also continue to work effectively at high temperatures, effectively extending the service life of the catalyst and reducing the use of precious metals. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 TEM images of the nanoparticles in the embodiments and comparative examples are shown. Specifically, Figure 1 (A) shows the Pd@CeO2 nanoparticles in Examples 1 and 2; Figure 1 (B) shows the Pd@CeO2-OA nanoparticles in Examples 3 and 4; Figure 1 (C) shows the Pd-CeO2 nanoparticles in Comparative Examples 1 and 2; Figure 1 (D) shows the Pd—CeO 2 -OA nanoparticles in Comparative Examples 3 and 4.
[0042] Figure 2 TEM images of the catalysts of Examples 1-4 are shown, wherein Figure 2 (A) is the sample of Example 1, Figure 2 (B) is the sample of Example 2, Figure 2 (C) is the sample of Example 3, Figure 2 (D) is the sample of Example 4.
[0043] Figure 3 The graphs showing the change in CO conversion rate of the catalysts of Examples 1-4 and Comparative Examples 1-4 with temperature are shown.
[0044] Figure 4 The graphs showing the change in CH4 conversion rate of the catalysts in Examples 1-4 and Comparative Examples 1-4 with temperature are shown.
[0045] Figure 5 The curve diagram of the change of NO conversion rate of the catalysts of Examples 1-4 and Comparative Examples 1-4 with temperature is shown.
[0046] Figure 6 The hydrothermal stability test results of the catalysts of Example 3 and Comparative Example 3 for CO oxidation (a), CH4 oxidation (b) and NO reduction (c) at 500°C after hydrothermal aging treatment are shown. DETAILED DESCRIPTION
[0047] The following examples, combined with the accompanying drawings, are intended to illustrate in detail the synthesis process and performance test of the core-shell structure catalyst of the present application, so as to clearly demonstrate the technical features and implementation methods of the present application.
[0048] Embodiment 1:
[0049] This embodiment describes the process of synthesizing core-shell structured nanoparticles in one step by a self-oxidation-reduction method assisted by the salting-out effect, and synthesizing a Pd@CeO2 / Al2O3 core-shell structured catalyst with a Pd content of 1% and a CeO2 content of 10% by an electrostatic attraction loading method. First, 1.2 g of KBr was weighed and dissolved in 80 mL of deionized water, and heated at 60°C for 10 minutes; then, 3.2 mL of a 62.5 mmol / L Na2PdCl4 aqueous solution and 8 mL of a 0.1 M Ce(NO3)3 aqueous solution (formed by hexahydrated cerium nitrate) were added to the solution in sequence; then, 20 mL of a 0.15 mol / L ammonia aqueous solution was slowly added, and the reaction continued at 60°C for 1 hour; after the reaction was completed, it was cooled to room temperature, centrifuged and washed three times with deionized water to remove residual reaction by-products, and finally vacuum dried at 60°C overnight to obtain Pd@CeO2 core-shell structured nanoparticles.
[0050] Next, 1 g of γ-Al2O3 powder was dispersed in 100 mL of deionized water containing 400 μL of 25% ammonia water and heated at 95 °C for 2 hours to improve its surface properties; 100 mg of the Pd@CeO2 nanoparticles prepared above were dispersed in 10 mL of deionized water and ultrasonically treated, then slowly added to the pretreated γ-Al2O3 dispersion and continued to be heated at 95 °C for 2 hours to complete the loading; after cooling to room temperature, centrifugation was collected and vacuum dried at 60 °C overnight. The dried sample was then heated to 500 °C in an air atmosphere at a heating rate of 3 °C / min and kept warm for 3 hours for calcination; after cooling to room temperature, the final sample was labeled Pd@CA-E-500, with a Pd precious metal content of 1% and a CeO2 content of 10%.
[0051] Embodiment 2:
[0052] The method of this example is the same as that of Example 1, the only difference being that the calcination temperature is adjusted from 500°C to 850°C to evaluate the effect of different calcination conditions on the properties of the catalyst. A Pd@CeO2 / Al2O3 core-shell structure catalyst with a Pd noble metal content of 1% and a CeO2 content of 10% is obtained, which is labeled as Pd@CA-E-850.
[0053] Embodiment 3:
[0054] The present embodiment aims to synthesize oleic acid-modified Pd@CeO2 core-shell structured nanoparticles in one step by a self-oxidation-reduction method assisted by a salting-out effect, and to synthesize a Pd@CeO2 / Al2O3 core-shell structured catalyst with a Pd content of 1% and a CeO2 content of 10% by a supramolecular self-assembly loading method.
[0055] First, oleic acid-modified Pd@CeO2 core-shell structured nanoparticles were synthesized: Pd@CeO2 nanoparticles were synthesized according to the preliminary steps of Example 1 above. First, 1.2 g of KBr was weighed and dissolved in 80 mL of deionized water, and heated at 60°C for 10 minutes. Then, 3.2 mL of 62.5 mmol / L Na2PdCl4 aqueous solution and 8 mL of 0.1 M Ce(NO3)3 aqueous solution were added to the solution in sequence; then, 20 mL of 0.15 mol / L ammonia aqueous solution was slowly added; after ammonia was added dropwise to the reaction solution, 100 mL of CHCl3 solution containing 0.68 g of oleic acid was further added, and heated at 60°C for 30 minutes to promote the transfer of nanoparticles to the CHCl3 phase; then, the CHCl3 phase was separated and evaporated to obtain nanoparticle solids, which were washed with ethanol to remove free oleic acid, and finally vacuum dried at 60°C overnight to obtain oleic acid-modified Pd@CeO2 core-shell structured nanoparticles, marked as Pd@CeO2-OA.
[0056] Next, a hydrophobic Al2O3 carrier was prepared by weighing 2 g of γ-Al2O3 powder and ultrasonically treating it in 20 mL of ethanol. 1.10 mL of octyltrimethoxysilane (TEOOS) was added, and the mixture was refluxed at 85°C for 3 hours, washed by centrifugation, and dried in a vacuum at 60°C to obtain a hydrophobic Al2O3 carrier.
[0057] Subsequently, 1 g of the hydrophobic Al2O3 powder prepared above was dispersed in 15 mL of tetrahydrofuran (THF), and 100 mg of the Pd@CeO2-OA nanoparticles prepared above were added. After ultrasonic treatment, the mixture was stirred at room temperature overnight, centrifuged, washed, and dried in a vacuum at 60°C. The dried sample was heated to 500°C in an air atmosphere at a heating rate of 3°C / min and kept warm for 3 hours for calcination. After cooling to room temperature, the obtained sample was labeled Pd@CA-S-500, and its Pd precious metal content was 1% and the CeO2 content was 10%.
[0058] Embodiment 4:
[0059] The method of this example is the same as that of Example 3, the only difference being that the calcination temperature is adjusted from 500°C to 850°C to evaluate the effect of different calcination conditions on the properties of the catalyst. A Pd@CeO2 / Al2O3 core-shell structure catalyst with a Pd noble metal content of 1% and a CeO2 content of 10% is obtained, which is labeled as Pd@CA-S-850.
[0060] Comparative Example 1:
[0061] In this comparative example, a non-core-shell structure supported catalyst was prepared by a synthesis method similar to that of Example 1, except that inorganic salt KBr was not used in the synthesis process. This change was intended to explore the key role of inorganic salt KBr in the synthesis of core-shell structured nanoparticles.
[0062] The steps of Example 1 were followed, but the addition of KBr was omitted. First, 3.2 mL of 62.5 mmol / L Na2PdCl4 aqueous solution and 8 mL of 0.1 M Ce(NO3)3 aqueous solution were directly added to 80 ml of deionized water preheated to 60°C. Subsequently, 20 mL of 0.15 mol / L ammonia solution was slowly added, and the reaction was continued at 60°C for 1 hour. After the reaction was completed, it was cooled to room temperature, centrifuged and washed three times with deionized water to remove residual reaction by-products, and finally vacuum dried at 60°C overnight to obtain Pd-CeO2 nanoparticles without KBr-assisted synthesis.
[0063] Next, 1g of γ-Al2O3 powder was dispersed in 100mL of deionized water containing 400μL of 25% ammonia water and heated at 95°C for 2 hours to improve its surface properties; 100mg of Pd-CeO2 nanoparticles were dispersed in 10mL of deionized water and ultrasonically treated, then slowly added dropwise to the pretreated γ-Al2O3 dispersion, and continued to heat at 95°C for 2 hours to complete the loading. After cooling to room temperature, centrifugation was collected and vacuum dried at 60°C overnight. The dried sample was then heated to 500°C in an air atmosphere at a heating rate of 3°C / min and kept warm for 3 hours for calcination. After cooling to room temperature, the final sample was labeled Pd-CA-E-500, with a Pd precious metal content of 1% and a CeO2 content of 10%. Comparative Example 2:
[0064] The method of this comparative example is the same as that of comparative example 1, the only difference being that the calcination temperature is adjusted from 500°C to 850°C to evaluate the effect of different calcination conditions on the properties of the catalyst. A Pd-CeO2 / Al2O3 core-shell-free supported catalyst with a Pd noble metal content of 1% and a CeO2 content of 10% is obtained, which is marked as Pd-CA-E-850.
[0065] Comparative Example 3:
[0066] In this comparative example, oleic acid-modified Pd-CeO2 nanoparticles were prepared by a synthesis method similar to that of Example 3, and loaded on hydrophobic Al2O3 by a self-assembly method to obtain a non-core-shell structure supported catalyst, except that inorganic salt KBr was not used in the synthesis process. This change is intended to explore the key role of inorganic salt KBr in the synthesis of core-shell structure nanoparticles.
[0067] The steps of Example 3 were followed, but the addition of KBr was omitted. First, 3.2 mL of 62.5 mmol / L Na2PdCl4 aqueous solution and 8 mL of 0.1 M Ce(NO3)3 aqueous solution were directly added to 80 ml of deionized water preheated to 60°C. Subsequently, 20 mL of 0.15 mol / L ammonia solution was slowly added. After ammonia was added dropwise to the reaction solution, 100 mL of CHCl3 solution containing 0.68 g of oleic acid was further added and heated at 60°C for 30 minutes to cause the nanoparticles to transfer to the CHCl3 phase. Subsequently, the CHCl3 phase was separated and evaporated to obtain a nanoparticle solid, which was washed with ethanol to remove free oleic acid and finally dried in vacuo at 60°C overnight to obtain oleic acid-modified Pd-CeO2 nanoparticles, labeled as Pd-CeO2-OA.
[0068] Next, a hydrophobic Al2O3 carrier was prepared by weighing 2 g of γ-Al2O3 powder and ultrasonically treating it in 20 mL of ethanol. 1.10 mL of octyltrimethoxysilane (TEOOS) was added, and the mixture was refluxed at 85°C for 3 hours, washed by centrifugation, and dried in a vacuum at 60°C to obtain a hydrophobic Al2O3 carrier.
[0069] Subsequently, 1 g of the hydrophobic Al2O3 powder prepared above was dispersed in 15 mL of tetrahydrofuran (THF), 100 mg of Pd-CeO2-OA nanoparticles were added, and after ultrasonic treatment, the mixture was stirred at room temperature overnight, centrifuged, washed, and dried in vacuum at 60°C. The dried sample was heated to 500°C in an air atmosphere at a heating rate of 3°C / min and kept at this temperature for 3 hours for calcination. After cooling to room temperature, the obtained sample was labeled Pd-CA-S-500, and its Pd precious metal content was 1% and CeO2 content was 10%.
[0070] Comparative Example 4:
[0071] The method of this comparative example is the same as that of comparative example 3, the only difference being that the calcination temperature is adjusted from 500°C to 850°C to evaluate the effect of different calcination conditions on the properties of the catalyst. A Pd-CeO2 / Al2O3 core-shell structure-free supported catalyst with a Pd noble metal content of 1% and a CeO2 content of 10% is obtained, which is marked as Pd-CA-S-850.
[0072] The morphology and structure of the nanoparticles prepared in the examples and comparative examples of the present application and the catalysts of Examples 1-4 were analyzed by transmission electron microscopy (TEM):
[0073] Figure 1 TEM images of the nanoparticles in the embodiments and comparative examples are shown. Specifically, Figure 1 (A) shows the Pd@CeO2 nanoparticles in Examples 1 and 2; Figure 1(B) shows the Pd@CeO2-OA nanoparticles in Examples 3 and 4; Figure 1 (C) shows the Pd-CeO2 nanoparticles in Comparative Examples 1 and 2; Figure 1 (D) shows the Pd-CeO2-OA nanoparticles in Comparative Examples 3 and 4; the test results show that the nanoparticles prepared by the method of the present application have an ideal core-shell structure, while the comparative examples do not have such an obvious structure; specifically, Figure 1 It can be seen from the TEM results that nanoparticles with a core-shell structure were successfully synthesized using the self-oxidation-reduction method assisted by the salting-out effect. The nanoparticles were mainly composed of a Pd core of approximately 10 nm in size and a CeO2 shell. The comparative example showed that the sample to which KBr was not added during the synthesis process did not show an obvious core-shell structure.
[0074] Figure 2 TEM images of the catalysts of Examples 1-4 are shown, wherein Figure 2 (A) is the sample of Example 1, Figure 2 (B) is the sample of Example 2, Figure 2 (C) is the sample of Example 3, Figure 2 (D) is the sample of Example 4; Figure 2 It can be seen from the TEM results that the catalysts loaded with core-shell nanoparticles on alumina carriers maintained a stable core-shell structure after calcination, demonstrating their good thermal stability.
[0075] Catalyst activity evaluation method:
[0076] The catalyst performance test method adopts standardized steps: first, 60 mg of catalyst is mixed with 540 mg of silica and placed in a reaction tube to ensure uniform distribution (the catalyst is fixed at both ends with quartz wool with a diameter of 3 to 5 μm to prevent flow). The temperature of all gas pipelines is set to 150°C to prevent water vapor condensation from affecting the experimental results. The test was carried out in a mixed gas flow containing 1000ppm CH4, 5000ppm CO, 1000ppmNO, 10% CO2, 0.4% O2 (balance is N2), with a total flow rate of 100mL / min, equivalent to a space velocity SV = 100L·g -1 ·h -1 , ensuring the air-fuel ratio λ = 1. During the experiment, the changes in the reaction gas components were monitored online by gas chromatograph (GC) and Fourier transform infrared gas analyzer (FTIR) to evaluate the catalyst's conversion efficiency of CH4, CO, and NO. By analyzing the conversion efficiency of the catalyst under different conditions and combining the experimental data, the performance of the catalyst and its application potential in natural gas vehicle exhaust purification were comprehensively evaluated.
[0077] Catalyst hydrothermal stability test method:
[0078] Hydrothermal aging treatment was performed to simulate the durability acceleration test under the driving conditions of compressed natural gas (CNG) heavy-duty vehicles. The samples were aged at 800°C for 16 hours in an oxidizing atmosphere containing 2.0% O2 and 10% H2O. Subsequently, the aged samples were heated at 500°C and a space velocity (WHSV) of 100 L·g -1 ·h -1 The stability test was conducted for 24 hours under the conditions of 1000ppm CH4, 5000ppm CO, 1000ppm NO, 4000ppm O2, 10% CO2 and 10% H2O, with N2 as the balance gas and a total flow rate of 100mL / min.
[0079] Table 1 Performance test data of the conversion rate of various pollutants of catalysts in different embodiments and comparative examples
[0080]
[0081] According to Table 1 and Figure 3 ( Figure 3 The data analysis of the curves of the change of CO conversion rate of the catalysts of Examples 1-4 and Comparative Examples 1-4 with temperature is shown. The Examples 1-4 and Comparative Examples 1-4 involved in the present application have good conversion efficiency for CO. By comparing Table 1, Figure 4 (showing a curve diagram showing the change in CH4 conversion rate of the catalysts of Examples 1-4 and Comparative Examples 1-4 with temperature) and Figure 5 (showing the curve of the change of NO conversion rate with temperature for the catalysts of Examples 1-4 and Comparative Examples 1-4), it can be clearly seen that the catalytic performance of the core-shell structure three-way catalysts in Examples 1-4 in CH4 oxidation and NO reduction is significantly better than that of the corresponding supported catalysts in Comparative Examples 1-4. In particular, the T90 values of the core-shell structure three-way catalyst Pd@CA-S-500 in Example 3 for CH4 oxidation and NO reduction reached 471°C and 443°C, respectively, which were 113°C and 177°C lower than those of the supported three-way catalyst Pd-CA-S-500 in Comparative Example 3. This result further proves the significant advantages of the core-shell structure three-way catalyst of the present application in improving the three-way catalytic activity, highlighting the key role of the core-shell structure in enhancing catalytic performance.
[0082] Figure 6The results of the 24-hour hydrothermal stability test of the catalysts of Example 3 Pd@CA-S-500 and Comparative Example 3 Pd-CA-S-500 at 500°C after hydrothermal aging treatment at 800°C for 16 hours are shown. After this test, the catalyst of Example 3 exhibited excellent anti-sintering and hydrothermal stability, and the catalytic conversion rate of CO, CH4 or NO remained at nearly 100%. In contrast, the conversion rate of CH4 and NO of the catalyst of Comparative Example 3 decreased significantly during the test, and the conversion rate was only maintained at less than 50% and 40%. This comparison clearly demonstrates the excellent hydrothermal stability and excellent anti-agglomeration and sintering ability of the core-shell structure three-way catalyst of the present application.
[0083] The discussion of the above embodiments and comparative examples is intended to explain in detail the unique advantages and application potential of the core-shell structure three-way catalyst of the present application in improving the exhaust purification efficiency of natural gas vehicles. It should be emphasized that these examples are only to more clearly illustrate the technical features of the present application, rather than to limit the scope of protection of the present application. Ordinary technicians in the technical field can make various forms of changes, modifications or equivalent substitutions without departing from the spirit and principles of the present application, and these changes, modifications or equivalent substitutions should be included in the scope of protection of the present application.
Claims
1. A hydrothermally stable core-shell three-way catalyst, characterized in that: The catalyst consists of a core-shell structure containing active components and a carrier material, wherein the core-shell structure is loaded into the carrier material; the core component of the core-shell structure is a precious metal, and its content is 0.1-5wt% of the total weight of the catalyst; the shell component of the core-shell structure is a solid solution or a combination thereof, and its content is 10-60wt% of the total weight of the catalyst, and the remainder is the carrier material.
2. The hydrothermally stable core-shell three-way catalyst according to claim 1, characterized in that: The noble metal is one of Pd, Rh, Pt, Au or a combination thereof; the shell component is selected from zirconium oxide, cerium dioxide, cerium-zirconium solid solution or a combination thereof; the carrier material includes one or a combination of oxygen storage material and / or alumina or cerium-aluminum solid solution; the catalyst loading method includes electrostatic attraction and supramolecular self-assembly method.
3. The hydrothermally stable core-shell three-way catalyst according to claim 2, characterized in that: The content of the noble metal is 0.5-2wt% of the total weight of the catalyst; the content of the cerium dioxide is 10wt% to 40wt%, and the content of the zirconium oxide is 10 to 20wt%; the carrier material can be doped with structural additives BaO, La2O3 or Y2O3, and the content is 3-10wt% of the total catalyst.
4. The hydrothermally stable core-shell three-way catalyst according to claim 2, characterized in that: The noble metal is Pd; the shell component is cerium dioxide; and the carrier material is aluminum oxide.
5. A method for preparing a hydrothermally stable core-shell three-way catalyst according to claims 1-4, characterized in that: The preparation steps include: (1) Synthesis of core-shell structured nanoparticles: A noble metal precursor and a shell material precursor are added by an inorganic salt-assisted self-oxidation-reduction method, and then ammonia water is added, followed by heating, centrifugal washing and drying to obtain core-shell structured nanoparticles; (2) Preparation and surface modification of the carrier: the carrier powder is dispersed in aqueous ammonia and heated to improve the surface properties of the carrier; or the carrier powder is mixed with octyltrimethoxysilane, and the mixture is refluxed, centrifuged and dried to obtain a hydrophobic carrier; (3) Core-shell structure supported catalyst: the carrier powder of step (2) is dispersed and heated in an aqueous solution containing ammonia or a tetrahydrofuran solution, and then the core-shell structure nanoparticles are added to the reaction system and continue to be heated, and finally centrifugally dried to obtain a catalyst powder; (4) Heat treatment: The catalyst powder obtained in step (3) is calcined for 3-6 hours to obtain a three-way catalyst.
6. The method for preparing a hydrothermally stable core-shell three-way catalyst according to claim 5, characterized in that: The inorganic salt described in step (1) is at least one of KBr, KCl, and KI; the precious metal precursor described in step (1) includes one or more of sodium tetrachloropalladate, potassium chloroplatinite, and rhodium trichloride trihydrate; the shell material precursor described in step (1) is a soluble salt solution of one or more of cerium nitrate hexahydrate, cerium acetate, and zirconium nitrate; the carrier powder described in step (2) is a mixture of oxygen storage material and aluminum oxide or a combination of one or more of cerium aluminum solid solutions.
7. The method for preparing a hydrothermally stable core-shell three-way catalyst according to claim 6, characterized in that: The precious metal precursor described in step (1) is sodium tetrachloropalladate; the shell material precursor described in step (1) is cerium nitrate hexahydrate; the core-shell structure nanoparticles described in step (1) also include oleic acid modification, specifically: after the ammonia water is added dropwise, an oleic acid solution mixed in CHCl3 is added to the reaction system for modification.
8. The method for preparing a hydrothermally stable core-shell three-way catalyst according to claim 7, characterized in that: When the core-shell structured nanoparticles described in step (4) are oleic acid-modified core-shell structured nanoparticles, the hydrophobic carrier is dispersed in a tetrahydrofuran solution.
9. The method for preparing a hydrothermally stable core-shell three-way catalyst according to claim 8, characterized in that: The carrier powder described in step (2) is γ-phase activated alumina; the loading method of the core-shell structure loaded catalyst described in step (3) includes electrostatic attraction and supramolecular self-assembly method; the calcination conditions described in step (4) are a muffle furnace heating rate of 3°C / min, and a calcination temperature set to 500°C or 850°C.
10. An application of the hydrothermally stable core-shell three-way catalyst according to any one of claims 1 to 4, characterized in that: The catalyst is suitable for treating harmful gases in high-temperature exhaust gas, and is particularly suitable for exhaust gas purification of compressed natural gas engines.
Citation Information
Patent Citations
Zinc oxide or nickel oxide photocatalyst and preparation method thereof
CN115301223A
Platinum-rhodium catalyst for automobile waste gas
JP2006116460A