Preparation method and application of microporous SiO2 modified MOF (Metal Organic Framework) derived ferrocobalt composite material

By coating mesoporous SiO2 on the surface of Fe-ZIF 67 and calcining to form a microporous SiO2-modified MOF-derived cobalt-iron composite catalyst, the problem of poor stability of MOF-derived cobalt material is solved, and the effect of efficient degradation of antibiotic pollutants is achieved.

CN118988319AActive Publication Date: 2024-11-22YANGTZE ECOLOGY & ENVIRONMENT CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411100337.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

The existing MOF-derived cobalt materials have poor stability and easy agglomeration in terms of catalytic properties, making it difficult to effectively remove antibiotic pollutants in water bodies.

Method used

Catalytic activity and structural stability are improved by coating mesoporous SiO2 on the surface of the precursor Fe-ZIF 67 and forming microporous SiO2-modified MOF-derived cobalt-ferrobimetal composite catalyst CoFeCMs@mSiO2 by water etching and calcination.

Benefits of technology

It significantly improves the stability and catalytic performance of the catalyst, can efficiently degrade ofloxacin, with a degradation rate of 88.9%-91.7%, and maintains a high efficiency during recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988319A_ABST
    Figure CN118988319A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a microporous SiO2 modified MOF derived ferrocobalt composite material, mesoporous SiO2 is coated with a precursor Fe-ZIF 67, CoFeCMs (at) mSiO2 with a core-shell structure is formed after calcination, the catalyst has a large specific surface area and excellent catalytic performance, and the specific surface area can reach 274.82 m < 2 > / g. The catalyst can generate more exposed active sites, PMS can be efficiently activated, and a CoFeCMs (at) mSiO2 / PMS system can effectively degrade 91.7% of OFX with the concentration of 20 mg / L within 20 min. According to the invention, more choices are provided for application of the MOF-derived bimetallic-based composite material as AOPs to degradation of organic pollutants.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of antibiotic treatment of organic pollution, and in particular to a preparation method and application of a microporous SiO2-modified MOF-derived cobalt-iron composite material. Background Art

[0002] In the past few decades, antibiotics have played an important role in treating human and animal diseases and promoting the growth and development of livestock. However, only part of the antibiotics can be metabolized and absorbed by humans or animals, and the rest is discharged into the aquatic environment through feces or urine. Their continued presence in the aquatic environment makes bacteria in the water highly resistant, which seriously threatens the aquatic environment and human health.

[0003] Traditional AOPs technology based on ·OH is non-selective for the mineralization pathway of organic matter and generally needs to be carried out in a highly acidic environment. The SR-AOPs process has universal applicability and high efficiency in disinfection and removal of new pollutants. Pollutants in the environment are mineralized into small molecules through AOPs technology, and finally exist in the form of CO2 and H2O. SR-AOPs technology has gradually replaced traditional AOPs technology based on ·OH to some extent, mainly due to ①SO4 ·- The redox potential of SO4 is 2.5-3.1V, which is higher than that of OH, 1.8-2.7V; ·- High stability and long half-life; ③ It can efficiently remove many pollutants; ④ In a wide pH range, SO4 ·- Can effectively remove pollutants; ⑤ Economical, efficient and environmentally friendly.

[0004] MOF-derived materials retain the advantages of MOF materials such as three-dimensional pore structure, large specific surface area, abundant active sites, adjustable metal elements and pore structure, and are a promising SR-AOPs catalyst. Cobalt is considered to be the most effective transition metal for SR-AOPs to remove organic pollutants. However, the catalytic performance of MOF-derived cobalt-based metal materials is limited, and there are problems such as easy agglomeration and poor stability. MOF-derived cobalt-iron bimetallic materials promote the 3+ / Co 2+ , Fe 3+ / Fe 2+ The redox cycle of the catalyst enhances the catalytic performance.

[0005] The yolk-shell structure has attracted great interest due to its unique structure and wide application in different fields. In particular, the yolk-shell catalyst has the following obvious advantages: the active nanoparticles are stabilized by encapsulation; the microenvironment formed by the yolk-shell structure provides a reaction driving force for adsorption and degradation; the active sites can be designed in the core part or embedded in the gap to improve stability while retaining its entire surface active sites. SiO2 as a shell can improve the stability of the material and also play a protective role during the calcination process.

[0006] In summary, the microporous SiO2-modified MOF-derived cobalt-iron composites show great potential in activating PMS to degrade antibiotics in water. As a highly efficient catalyst in advanced oxidation technology, the microporous SiO2-modified MOF-derived cobalt-iron composites will surely have great application value in future wastewater treatment. Summary of the invention

[0007] The purpose of the present invention is to provide a preparation method and application of a microporous SiO2-modified MOF-derived cobalt-iron composite material, by coating mesoporous SiO2 on the surface of the precursor Fe-ZIF 67, and then forming a microporous SiO2-modified MOF-derived cobalt-iron bimetallic composite catalyst CoFeCMs@mSiO2 by water etching and calcination. The cobalt-iron bimetallic derived from MOF can improve the catalytic activity and structural stability through synergistic effects, and SiO2 as a shell can improve the stability of the material.

[0008] To achieve the above object, the technical solution adopted by the present invention is:

[0009] A method for preparing a microporous SiO2-modified MOF-derived cobalt-iron composite material comprises the following steps:

[0010] Step 1: Prepare the precursor Fe-ZIF 67 by co-precipitation method:

[0011] 10 mL of 1 mol / L NaOH and 10 mL of 3.36 mol / L 2-methylimidazole solution were mixed and stirred evenly, and the mixture was ultrasonicated for 10 min. The prepared solution was referred to as solution A.

[0012] Take 0.8 mL of 0.8 mol / L Co(NO3)2·6H2O and 9.6 mL of 0.1 mol / L FeCl3·6H2O solution, mix them evenly, dilute them to 12 mL with water, and use ultrasonic for 10 min as solution B.

[0013] Under stirring conditions, solution B was slowly added dropwise to solution A. After the addition was completed, stirring was continued at room temperature for 24 hours. The mixed solution was centrifuged to collect the solid matter. The solid matter was then repeatedly washed with water and methanol alternately for several times and dried at 60° C. to obtain the precursor Fe-ZIF 67. The molar ratio of Co element to Fe element in the precursor Fe-ZIF 67 was 1:1.5.

[0014] Step 2: Preparation of Fe-ZIF 67@mSiO2:

[0015] The precursor Fe-ZIF 67 prepared in step 1 is dispersed in water to prepare a Fe-ZIF67 aqueous solution with a concentration of 1 mg / mL. 100 mL of the Fe-ZIF 67 aqueous solution is mixed with 20 mL of a 62.5 mg / mL hexadecyltrimethylammonium bromide ethanol solution and stirred for 1 h. The mixed solution is heated to 50°C, 0.5 mL of ammonia water is added, 583 mg of tetraethyl silicate is mixed with 10 mL of ethanol and then added dropwise to the mixed solution several times, and stirred vigorously at 50°C for 6 h. After the reaction is completed, the solution is centrifuged, the solid is collected, the solid is washed three times with ethanol, and dried at 60°C to obtain Fe-ZIF 67@mSiO2.

[0016] Step 3: Preparation of Fe-ZIF 67@mSiO2 after removal of hexadecyltrimethylammonium bromide and water etching

[0017] The Fe-ZIF 67@mSiO2 prepared in step 2 is extracted with an ethanol solution of ammonium nitrate at 80°C to remove hexadecyltrimethylammonium bromide in the shell structure of Fe-ZIF 67@mSiO2;

[0018] After removing the hexadecyltrimethylammonium bromide, Fe-ZIF 67@mSiO2 was dispersed in water at a concentration of 2 mg / mL, and 70 mL of the dispersion was loaded into a 100 mL reactor and kept at 100 °C for 24 h.

[0019] The dispersion was centrifuged and the solid was collected, washed with ethanol, and dried at 60°C to obtain Fe-ZIF 67@mSiO2 after removal of hexadecyltrimethylammonium bromide and water etching;

[0020] Step 4: Calcination in air atmosphere to prepare CoFeCMs@mSiO2

[0021] The Fe-ZIF 67@mSiO2 prepared in step 3 after removal of hexadecyltrimethylammonium bromide and water etching was ground into powder, placed in a tube furnace at 500-600°C, and calcined for 2 hours in an air atmosphere to obtain a microporous SiO2-modified MOF-derived cobalt-iron composite material CoFeCMs@mSiO2.

[0022] Preferably, in step 2, tetraethyl silicate is added dropwise to the mixed solution in 5 portions.

[0023] Preferably, the centrifugal speed of the solution in step 1 and step 2 is 8000 rpm.

[0024] Preferably, the heating rate of the tube furnace in step 4 is 5°C / min.

[0025] An application of a microporous SiO2-modified MOF-derived cobalt-iron composite material. The microporous SiO2-modified MOF-derived cobalt-iron composite material CoFeCMs@mSiO2 is used to activate peroxymonosulfate to degrade ofloxacin.

[0026] Preferably, the degradation method is as follows: 100 mL of a 20-30 mg / L ofloxacin solution is put into a 1000 mL beaker, the beaker is placed on a shaker for shaking, 0.04-0.05 g of a microporous SiO2-modified MOF-derived cobalt-iron composite material CoFeCMs@mSiO2 and 0.03-0.04 g of peroxymonosulfate are added to the beaker, and the peroxymonosulfate is activated by the synergistic effect of the cobalt-iron bimetallic in the MOF-derived cobalt-iron composite material CoFeCMs@mSiO2 to degrade ofloxacin; the degradation time is 20 min, 2-3 mL of the solution in the degradation process is taken out with a syringe, the solution is filtered with a 0.22 μm polyethersulfone PES filter membrane and then placed in a quartz cuvette, and the ofloxacin concentration is analyzed by UV-Vis at a wavelength of 294 nm, and the degradation rate of ofloxacin is 88.9%-91.7%.

[0027] Characterization of microporous SiO2-modified MOF-derived cobalt-iron composite CoFeCMs@mSiO2 catalysts:

[0028] 1. Characterization of microscopic morphology

[0029] like Figure 2 As shown in (a), the surface of the synthesized precursor Fe-ZIF 67 is relatively smooth and has the dodecahedral structure of ZIF; Figure 2 (b) The surface of Fe-ZIF 67 is coated with mesoporous SiO2 to form spherical nanoparticles with a particle size of about 300-600nm; Figure 2 (c) is the SEM image of CoFeCMs without mesoporous SiO2 and after calcination. It can be seen that the structure collapses very seriously and the cobalt-iron bimetallic oxide is deposited on the surface, making the surface rough. Figure 2 The TEM image in (d) shows the core-shell structure formed by the mesoporous SiO2 coating, which still has a complete core-shell structure after calcination; Figure 2In (e), HRTEM measured a lattice spacing of 0.254 nm, corresponding to the (311) plane of CoFe2O4.

[0030] 2. XRD analysis

[0031] Figure 3 (a) is the XRD spectrum of Fe-ZIF 67, Fe-ZIF 67@mSiO2, CoFeCMs@mSiO2, and CoFeCMs. The characteristic peaks of SiO2 at 22.0° and 36.4° correspond to the (101) and (112) crystal planes of SiO2, respectively, and the characteristic peak at 33.1° corresponds to the (104) crystal plane of Fe2O3. The characteristic diffraction peaks at 35.7° and 53.8° in CoFeCMs@mSiO2 and CoFeCMs correspond to the (311) and (422) crystal planes of SiO2, respectively, which correspond to the characteristic peaks of spinel structure CoFe2O4. In addition, there are two other characteristic peaks of CoFe2O4 in CoFeCMs, located at 37.3° and 62.7°, corresponding to the (222) and (440) crystal planes. The SiO2 characteristic peaks at 22.0° and 36.4° of Fe-ZIF 67@mSiO2 and CoFeCMs@mSiO2 weakened, which was caused by the decomposition of part of silica after calcination; Figure 3 (b) shows that the higher the calcination temperature, the stronger the characteristic peak of CoFe2O4, indicating that more CoFe2O4 is formed; based on the above analysis, it is confirmed that SiO2 and CoFe2O4 components exist in CoFeCMs@mSiO2, combined with SEM analysis, indicating the successful coating of SiO2.

[0032] 3. XPS analysis

[0033] The chemical state and surface element composition of CoFeCMs@mSiO2 were analyzed using XPS spectroscopy. Figure 4 (a) It can be seen that the prepared material contains C, O, Si, Fe and Co elements; Figure 4 The three peak binding energies in (b) are 284.8 eV, 286.6 eV, and 288.1 eV, which correspond to -CC, -CO, and OCO, respectively. Before the catalytic reaction, the proportions of -CC, -CO, and OCO are 74.39%, 19.65%, and 5.96%, respectively, and after the reaction, they are 72.72%, 21.44%, and 5.94%, respectively. Figure 4The three peaks in (c) are at 532.4eV, 533.0eV and 533.8eV, which belong to lattice oxygen, adsorbed oxygen and surface adsorbed water, respectively. The binding energy of 532.4eV is attributed to Fe-O / Co-O, and the peak at 533.0eV comes from the CO peak, which corresponds to 286.6eV in the C1s spectrum. It may be that the carbon skeleton of MOF has been partially oxidized. Before the catalytic reaction, the contents of lattice oxygen, adsorbed oxygen and surface adsorbed water were 51.21%, 29.70% and 19.09%, respectively, and after the reaction, they were 50.48%, 23.55% and 25.97%, respectively, indicating that O participated in the redox process of iron and cobalt ions. Figure 4 A peak at 103.6 eV in (d) comes from SiO2; Figure 4 In (e), the peaks of the Fe 2p spectrum at 711.1 eV / 724.0 eV belong to Fe 2+ (2p 3 / 2 / 2p 1 / 2 ), 714.1eV / 726.6eV belongs to Fe 3+ (2p 3 / 2 / 2p 1 / 2 ), 718.6eV belongs to the satellite peak, Fe 2+ / Fe 3+ The increase from 1.27 to 2.07 indicates that Fe 2+ / Fe 3+ Participated in the degradation process; Figure 4 In (f), the peaks at 782.1eV / 797.8 and 785.5eV / 800.0eV of the Co 2p spectrum are Co 2+ (2p 3 / 2 / 2p 1 / 2 ) and Co 3+ (2p 3 / 2 / 2p 1 / 2 ), the peaks at 787.4eV and 803.7 are satellite peaks; Co 2+ / Co 3+ The decline from 2.37 to 2.23 indicates that Co 2+ / Co 3+ Participated in the degradation process. Combining the above SEM, TEM and XRD analysis results, it can be seen that CoFeCMs@mSiO2 with core-shell structure was successfully prepared.

[0034] 4. Raman analysis

[0035] In Raman spectroscopy, the D band and G band indicate the presence of defects in the carbon skeleton and the presence of sp 2 Hybridized carbon atoms. Figure 5 As shown in Figure 2, the peaks at 1580 cm in CoFeCMs@mSiO2 and CoFeCMs -1The G band peak nearby is relatively low, which may be due to the less obvious stretching vibration of the carbon atom in-plane bond; -1 The D band peak near CoFeCMs is significantly stronger than that of CoFeCMs@mSiO2, which indicates that the density of disordered carbon and carbon defects in CoFeCMs is higher than that in CoFeCMs@mSiO2. Based on the above analysis, it can be seen that after calcination of Fe-ZIF 67 coated with mesoporous SiO2, the carbon defect density is lower than that of Fe-ZIF 67 directly calcined, and mesoporous SiO2 plays a protective role during the calcination process.

[0036] 5. N2 adsorption curve and BET analysis

[0037] Table 1 shows the BET test data of Fe ZIF-67, CoFeCMs and CoFeCMs@mSiO2. Figure 6 (a) and Table 1 show that the specific surface area of ​​Fe-ZIF 67 is 820.35 m 2 / g, the specific surface area of ​​CoFeCMs@mSiO2 coated with mesoporous SiO2 and calcined is 274.82m 2 / g, the specific surface area of ​​CoFeCMs formed by direct calcination is only 22.97m 2 / g; After calcination, the specific surface area of ​​Fe-ZIF 67 will decrease, which is caused by the loss of the carbon skeleton of Fe-ZIF 67 during the calcination process, but the specific surface area of ​​CoFeCMs@mSiO2 is much higher than that of CoFeCMs; Figure 6 In (a), the N2 adsorption-desorption isotherms of Fe-ZIF 67, CoFeCMs@mSiO2 and CoFeCMs are the IV isotherms of the H3 hysteresis loop, indicating the existence of mesopores inside them; the pore size distribution of Fe-ZIF 67 and CoFeCMs@mSiO2 is around 2-10nm, mainly concentrated around 5nm, and the pore size of CoFeCMs is relatively large, basically concentrated in 10-30nm, but the pore volume is small.

[0038] Table 1

[0039]

[0040] The catalytic degradation of ofloxacin by the microporous SiO2-modified MOF-derived cobalt-iron composite material CoFeCMs@mSiO2 prepared by this method:

[0041] The target pollutants are calculated as follows:

[0042] Among them, R t represents the degradation rate at time t, C0 and C t represent the concentration of pollutants and the concentration of pollutants at time point t respectively.

[0043] 1. Effect of calcination temperature on the degradation of ofloxacin OFX

[0044] During the formation of MOF-derived materials, the calcination temperature has an important influence on the structure and catalytic performance of the materials. Therefore, this experiment investigated the effect of CoFeCMs@mSiO2 calcined at 300℃, 400℃, 500℃, 600℃, and 700℃ on the degradation of OFX. Figure 7 As shown in the figure, the removal rate of OFX by CoFeCMs@mSiO2 at 300-600℃ was kept at about 90% within 20min, but the removal rate within 1min was significantly different, with a faster removal rate at 500℃. The removal efficiency at 700℃ was 85.6%, but the degradation rate was slower, which may be due to the high temperature during calcination, which severely damaged the carbon skeleton of the ZIF structure, resulting in a small number of active sites, a limited number of active species, and a slow degradation rate of OFX.

[0045] 2. Effects of different catalyst systems on OFX degradation

[0046] In order to explore the core-shell structure of CoFeCMs@mSiO2 formed by coating mSiO2, the outer shell mSiO2 can reduce the loss of carbon skeleton during calcination and make it have more active sites. The degradation performance of CoFeCMs@mSiO2 and CoFeCMs on OFX was compared. Figure 8 As shown in (a), without adding PMS, the degradation rates of OFX by CoFeCMs@mSiO2 and CoFeCMs were 54.9% and 11.3%, respectively. It can be seen that the degradation rate of the composite catalyst after coating and calcination was significantly improved. After adding 0.3g / L PMS, CoFeCMs@mSiO2 / PMS and CoFeCMs / PMS systems removed 91.7% and 35.6% of OFX, respectively, within 20min. It is worth noting that CoFeCMs@mSiO2 / PMS can efficiently degrade 88.7% of OFX within 3min. Figure 8 As shown in (b), the reaction kinetic constants of CoFeCMs@mSiO2 / PMS and CoFeCMs / PMS systems were calculated to be 0.255min -1 and 0.55min -1 , the rate constant of CoFeCMs@mSiO2 / PMS system is approximately CoFeCMs / PMS system. Based on the above analysis, it is confirmed that the material coated with mSiO2 has better catalytic degradation performance.

[0047] 3. Effect of different initial pH on OFX degradation

[0048] The initial pH of the solution has a certain influence on the generation of free radicals and the morphological changes of organic matter. Therefore, the effect of initial pH on the removal of OFX in the CoFeCMs@mSiO2 / PMS system was studied. Fig. 9 It can be seen that when the pH value gradually increases from 3 to 7, the removal rate of OFX increases continuously, and the degradation rates at pH values ​​of 3, 5, and 7 are 84.6%, 88.2%, and 91.7%, respectively. ·- and OH will react with H + The reaction generates less active HSO4 - Or directly remove (3-1—3-3). When the pH gradually increases from 7 to 11, the degradation efficiency of OFX decreases significantly, from 91.7% to 34.7%. Under higher pH conditions, M(Ⅲ) is reduced to M(Ⅱ), which inhibits the generation of active species (3-4, 3-5), resulting in a significant decrease in the removal rate of OFX. Based on the above analysis, the degradation effect of OFX is best under neutral or weakly acidic conditions. In this experiment, pH = 7 was selected as the optimal pH.

[0049] M(Ⅱ) + H2O → MOH + + H + (3-1)

[0050]

[0051] OH + H + + e + → H2O (3-3)

[0052]

[0053] 4. Effect of peroxymonosulfate PMS dosage on OFX degradation

[0054] CoFeCMs@mSiO2 activates peroxymonosulfate PMS to produce active species and mineralizes to remove OFX. Therefore, the dosage of PMS plays a crucial role in the degradation of OFX by the system. Fig.10 As shown in the figure, when the PMS dosage increases from 0.1g / L to 0.3g / L, the degradation efficiency of OFX gradually increases, and the removal rate within 20min is basically maintained at about 90%, but the degradation efficiency within 3min gradually increases. When the PMS dosage is 0.3g / L, the removal efficiency of OFX is 91.7% within 20min. With the increase in the PMS dosage, the number of active species produced in the system increases relatively, which accelerates the removal of OFX. When the PMS dosage continues to increase from 0.3g / L, the degradation efficiency within 20min does not change significantly, but the degradation efficiency within 3min decreases slightly, which indicates that when the amount of PMS reaches equilibrium with the amount of catalyst, SO4·- Free radicals will undergo self-quenching reaction. Based on the above analysis, 0.3g / L was used as the optimal dosage of PMS in this experiment.

[0055] 5. Effect of catalyst dosage on OFX degradation

[0056] In order to investigate the effect of catalyst dosage on the activation of PMS, different amounts of CoFeCMs@mSiO2 were used; e.g. Fig.11 As shown in the figure, when the catalyst increases from 0.2g / L to 0.4g / L, the OFX removal rate increases gradually within 20min. At 0.4g / L, the OFX degradation efficiency is 91.7%. When the catalyst amount continues to increase, the OFX removal rate does not increase significantly. Considering the catalytic degradation effect and operating cost, 0.4g / L is selected as the optimal catalyst dosage in this experiment.

[0057] 6. Effect of initial OFX concentration on OFX degradation

[0058] The experiment investigated the effect of the concentration of the target pollutant OFX solution on the degradation performance of the catalyst CoFeCMs@mSiO2. Fig.12 As shown in the figure, when the initial concentration of OFX is 10 mg / L, 20 mg / L and 30 mg / L, the removal rate of OFX within 20 min is 92.0%, 91.7% and 88.9% respectively. This shows that as the initial concentration of OFX increases, the degradation efficiency decreases. This is because the quantitative PMS and catalyst in the system have a limited number of active sites, and OFX molecules in the OFX solution with a higher concentration will compete for active species, resulting in a decrease in the reaction rate.

[0059] 7. Effect of actual water on OFX degradation

[0060] In order to explore the effect of actual water on OFX degradation, this experiment conducted a comparative study on OFX solutions made of ultrapure water, Yellow River water and tap water. Fig.13 As shown in the figure, the OFX degradation efficiencies of ultrapure water, Yellow River water, and tap water are 91.7%, 81.4%, and 79.7%, respectively. Yellow River water and tap water have a certain effect on the degradation of OFX. Combined with the effects of different ions on the degradation of OFX, the reduction in the degradation efficiency of OFX may be affected by HCO3 - and HPO4 2- The impact of plasma.

[0061] 8. Cyclic stability analysis

[0062] In order to explore the cycle stability of CoFeCMs@mSiO2 / PMS and CoFeCMs / PMS systems, 5 cycle tests were carried out. Fig.14As shown in (a), after 5 cycles, the degradation efficiency of CoFeCMs@mSiO2 / PMS for OFX decreased from 91.7% to 69.1% within 20 min. Fig.14 As shown in (b), the degradation efficiency of OFX by CoFeCMs / PMS system decreased from 35.6% to 9.5%. The removal rate of OFX by CoFeCMs@mSiO2 / PMS system reached 84.6% after the first three cycles. The degradation rate of OFX dropped sharply in the fourth and fifth cycles, which may be due to the blockage of some mSiO2 channels, which reduced the diffusion rate of OFX to CoFeCMs@mSiO2. However, the removal rate of OFX was still higher than that of bare CoFeCMs material. Fig.14 (c) is the XRD comparison diagram of CoFeCMs@mSiO2 and CoFeCMs before and after 5 cycles. It is found that the main diffraction peaks before and after the reaction have not changed, and are still consistent with the main diffraction peaks of CoFe2O4 with spinel structure, indicating that the crystal structure of the material has not changed. Fig.14 (d) and (e) show that the microstructure of the material has not changed significantly after 5 cycles. Based on the above analysis, the degradation efficiency and degradation rate of CoFeCMs@mSiO2 after 5 cycles are significantly higher than those of CoFeCMs, but the degradation efficiency of CoFeCMs@mSiO2 after 5 cycles is lower, which may be due to the blockage of the pores of mSiO2, which slows down the transfer rate between the active oxygen components and OFX.

[0063] 9. Degradation mechanism

[0064] (1) Determination of free radicals

[0065] In order to further identify the active species in the reaction system, free radical quenching experiments and EPR tests on the CoFeCMs@mSiO2 / PMS system using DMPO and TEMP spin traps were carried out. Fig.15 (a) Free radical quenching experiments were performed on the CoFeCMs@mSiO2 / PMS system to determine the contribution of different active species to the catalytic activity. ·- quencher), tert-butyl alcohol (TBA, quencher of ·OH), p-benzoquinone (p-BQ, O2 ·- quencher) and furfuryl alcohol (FFA, 1 After adding 10mM FFA to the system, the OFX degradation efficiency dropped to 31.3% in 20min. After adding methanol, the OFX removal rate dropped to 68.2%. After adding p-BQ and TBA, the OFX removal rates dropped to 75.7% and 87.4%, respectively. The corresponding contribution rate of the four active species to the catalytic activity is as follows: 1O2>SO4 ·- >O2 ·- >·OH, the main active species of CoFeCMs@mSiO2 / PMS degradation is 1 O2 and SO4 ·- .

[0066] like Fig.15 As shown in (b), (c), and (d), DMPO and TEMP were used to capture the active species in the detection system, and the active species in the system were captured at 1 min and 5 min. Fig.15 The signal peaks with peak intensity ratios of 1:2:2:1 and 1:1:1:1:1:1 in (b) correspond to DMPO-·OH and DMPO-SO4, respectively. ·- . Fig.15 The sextet in (c) is DMPO-O2 ·- signal. Fig.15 In (d), the signal peak with a peak intensity of 1:1:1 is TEMP- 1 O2 signal. Fig.15 (b), (c), and (d) show that there is SO4 in the CoFeCMs / PMS system. ·- , OH, O2 ·- , 1 O2 Four reactive oxygen species.

[0067] like Fig.16 As shown in the figure, the transfer of electrons from OFX to PMS was proved by the chronoamperometric test. With CoFeCMs@mSiO2 and CoFeCMs as working electrodes, it curve tests were carried out respectively. When PMS and OFX were added at 100s and 200s, respectively, it can be seen that the current changed significantly, indicating that when CoFeCMs@mSiO2 and CoFeCMs are used as media, electrons can be transferred from OFX to PMS through a non-radical pathway. In addition, the current of CoFeCMs@mSiO2 changed significantly at 100s and 200s, and there was significant electron transfer, while the current peak intensity of CoFeCMs was weak, indicating that CoFeCMs@mSiO2 has a stronger electron transfer ability.

[0068] (2) Degradation pathway of OFX

[0069] The intermediate substances in the OFX degradation process of CoFeCMs@mSiO2 / PMS system were determined by HPLC-MS, and the possible degradation pathways of OFX were analyzed. Fig.17As shown in the figure, the CN bond or CC bond of the piperazine ring of OFX is broken to generate the products P1 (m / z, 364), P2 (m / z, 336), P3 (m / z, 279) and P4 (m / z, 228). P3 is further decarboxylated and demorpholine-ringed to generate P5 (m / z, 116). OFX is first decarboxylated to generate P6 (m / z, 334), P6 is then dealkylated to generate P7 (m / z, 336), and then the piperazine ring is alkylated to generate P8 (m / z, 274). P8 is further 1 O2、SO4 ·- The oxidation of active free radicals such as hydroxylation, alkylation, and hydroxyl oxidation gradually generates P9 (m / z, 175) and P10 (m / z, 149). In general, the degradation pathway of OFX mainly involves several processes such as decarboxylation, hydroxylation, alkylation, and hydroxyl oxidation.

[0070] (3) Mechanism of OFX degradation by CoFeCMs@mSiO2 / PMS system

[0071] The degradation mechanism of OFX by CoFeCMs@mSiO2 / PMS system is as follows Fig.18 As shown, Co 3+ / Fe 3+ Reacts with PMS to generate sulfate radical SO5 ·- , SO5 ·- React with each other to produce SO4 ·- ,Co 2+ / Fe 2+ Reacts with PMS to generate SO4 ·- , O2 ·- It is made of SO5 ·- The O2 produced by the reaction gains an electron to form SO4 ·- ·OH is produced in the diffuse solution, and ·OH is in O2 ·- The reaction can generate 1 O2. Produced during the reaction 1 O2、SO4 ·- 、O2 ·- The ·OH attack destroys the structure of OFX, further mineralizing the pollutants into small molecules, CO2 and H2O. The entire reaction process is shown in Equations 3-6 to 3-12. In addition, the non-radical mechanism of CoFeCMs@mSiO2 also effectively promotes the transfer of electrons from OFX to PMS.

[0072]

[0073] In summary, the present invention forms CoFeCMs@mSiO2 with a core-shell structure by coating the precursor Fe-ZIF 67 with mesoporous SiO2 after calcination. The catalyst has a large specific surface area and excellent catalytic performance, and the specific surface area can reach 251.86 m 2 / g. This allows the catalyst to produce more exposed active sites, which can efficiently activate PMS, so that the CoFeCMs@mSiO2 / PMS system can effectively degrade 91.7% of OFX with a concentration of 20 mg / L within 20 minutes. The present invention provides more options for the application of MOF-derived bimetallic matrix composites as AOPs to degrade organic pollutants. BRIEF DESCRIPTION OF THE DRAWINGS

[0074] Figure 1 It is the synthesis route of CoFeCMs@mSiO2;

[0075] Figure 2 (a) is the SEM image of Fe-ZIF 67; (b) is the SEM image of CoFeCMs@mSiO2; (c) is the SEM image of CoFeCMs; (d) is the TEM image of CoFeCMs@mSiO2; (e) is the HRTEM image;

[0076] Figure 3 (a) is the XRD spectra of Fe-ZIF 67, Fe-ZIF 67@mSiO2, CoFeCMs@mSiO2, and CoFeCMs; (b) is the XRD spectra of CoFeCMs@mSiO2 at different calcination temperatures;

[0077] Figure 4 The XPS fine spectra of CoFeCMs@mSiO2 before and after the reaction: (a) full spectrum; (b) C 1s; (c) O 1s; (d) Si2p; (e) Fe 2p; (f) Co 2p;

[0078] Figure 5 is the Raman spectra of CoFeCMs@mSiO2 and CoFeCMs;

[0079] Figure 6 (a) is the N2 adsorption-desorption curves of Fe-ZIF 67, CoFeCMs@mSiO2 and CoFeCMs; (b) is the pore size distribution of Fe-ZIF67, CoFeCMs@mSiO2 and CoFeCMs;

[0080] Figure 7 is the effect of different calcination temperatures on the degradation of OFX (experimental parameters: [OFX] = 20 mg / L, [catalyst] = 0.4 g / L, [PMS] = 0.5 g / L);

[0081] Figure 8 is the effect of different catalytic systems on the degradation of OFX (experimental parameters: [OFX] = 20 mg / L, [catalyst] = 0.4 g / L, [PMS] = 0.3 g / L);

[0082] Fig. 9 is the effect of different initial pH on the degradation of OFX (experimental parameters: [OFX] = 20 mg / L, [catalyst] = 0.4 g / L, [PMS] = 0.3 g / L);

[0083] Fig.10 is the effect of PMS dosage on OFX degradation (experimental parameters: [OFX] = 20 mg / L, [catalyst] = 0.4 g / L, [pH] = 7);

[0084] Fig.11 is the effect of catalyst dosage on OFX degradation (experimental parameters: [OFX] = 20 mg / L, [PMS] = 0.3 g / L, [pH] = 7);

[0085] Fig.12 is the effect of the initial OFX concentration on the degradation of OFX (experimental parameters: [catalyst] = 0.4 g / L, [PMS] = 0.3 g / L, [pH] = 7);

[0086] Fig.13 is the effect of different water bodies on OFX degradation (experimental parameters: [OFX] = 20 mg / L, [catalyst] = 0.4 g / L, [PMS] = 0.3 g / L, [pH] = 7);

[0087] Fig.14 (a) 5-cycle stability test of CoFeCMs@mSiO2 / PMS system (experimental parameters: [OFX] = 20 mg / L, [catalyst] = 0.4 g / L, [PMS] = 0.3 g / L, [pH] = 7); (b) 5-cycle stability test of CoFeCMs / PMS system (experimental parameters: [OFX] = 20 mg / L, [catalyst] = 0.4 g / L, [PMS] = 0.3 g / L, [pH] = 7); (c) XRD comparison of CoFeCMs@mSiO2 and CoFeCMs before and after 5 cycles; (d) SEM image of CoFeCMs@mSiO2 after 5 uses; (e) SEM image of CoFeCMs after 5 uses;

[0088] Fig.15(a) Free radical quenching experiment (experimental parameters: [OFX] = 20 mg / L, [PMS] = 0.3 g / L, [catalyst] = 0.4 g / L, [pH] = 7), EPR spectrum of CoFeCMs@mSiO2 / PMS system: (b) DMPO-·OH and DMPO-SO4 ·- , (c)DMPO-O2 ·- , (d) TEMP- 1 O2;

[0089] Fig.16 are the chronoamperometric curves of CoFeCMs@mSiO2 and CoFeCMs;

[0090] Fig.17 It is the degradation pathway of OFX by CoFeCMs@mSiO2 / PMS system;

[0091] Fig.18 This is the reaction mechanism diagram of CoFeCMs@mSiO2 / PMS system to OFX. DETAILED DESCRIPTION

[0092] The present invention will be further described in detail below in conjunction with the accompanying drawings.

[0093] Example 1

[0094] A method for preparing a microporous SiO2-modified MOF-derived cobalt-iron composite material comprises the following steps:

[0095] Step 1: Prepare the precursor Fe-ZIF 67 by co-precipitation method:

[0096] 10 mL of 1 mol / L NaOH and 10 mL of 3.36 mol / L 2-methylimidazole solution were mixed and stirred evenly, and the mixture was ultrasonicated for 10 min. The prepared solution was referred to as solution A.

[0097] Take 0.8 mL of 0.8 mol / L Co(NO3)2·6H2O and 9.6 mL of 0.1 mol / L FeCl3·6H2O solution, mix them evenly, dilute them to 12 mL with water, and use ultrasonic for 10 min as solution B.

[0098] Solution B was slowly added dropwise to solution A under stirring. After the addition was completed, stirring was continued at room temperature for 24 hours. The mixed solution was centrifuged to collect the solid matter at a centrifugal rate of 8000 rpm. The solid matter was then repeatedly washed with water and methanol alternately for several times and dried at 60° C. to obtain the precursor Fe-ZIF 67. The molar ratio of Co element to Fe element in the precursor Fe-ZIF 67 was 1:1.5.

[0099] Step 2: Preparation of Fe-ZIF 67@mSiO2:

[0100] The precursor Fe-ZIF 67 prepared in step 1 is dispersed in water to prepare a Fe-ZIF67 aqueous solution with a concentration of 1 mg / mL. 100 mL of the Fe-ZIF 67 aqueous solution is mixed with 20 mL of a 62.5 mg / mL hexadecyltrimethylammonium bromide ethanol solution and stirred for 1 h. The mixed solution is heated to 50°C, 0.5 mL of ammonia water is added, 583 mg of tetraethyl silicate is mixed with 10 mL of ethanol and then added dropwise to the mixed solution in 5 times, and stirred vigorously at 50°C for 6 h. After the reaction is completed, the solution is centrifuged at a centrifugal rate of 8000 rpm. The solid matter is collected, washed three times with ethanol, and dried at 60°C to obtain Fe-ZIF67@mSiO2.

[0101] Step 3: Preparation of Fe-ZIF 67@mSiO2 after removal of hexadecyltrimethylammonium bromide and water etching

[0102] The Fe-ZIF 67@mSiO2 prepared in step 2 is extracted with an ethanol solution of ammonium nitrate at 80°C to remove hexadecyltrimethylammonium bromide in the shell structure of Fe-ZIF 67@mSiO2;

[0103] After removing the hexadecyltrimethylammonium bromide, Fe-ZIF 67@mSiO2 was dispersed in water at a concentration of 2 mg / mL, and 70 mL of the dispersion was loaded into a 100 mL reactor and kept at 100 °C for 24 h.

[0104] The dispersion was centrifuged and the solid was collected, washed with ethanol, and dried at 60°C to obtain Fe-ZIF 67@mSiO2 after removal of hexadecyltrimethylammonium bromide and water etching;

[0105] Step 4: Calcination in air atmosphere to prepare CoFeCMs@mSiO2

[0106] The Fe-ZIF 67@mSiO2 prepared in step 3 after removal of hexadecyltrimethylammonium bromide and water etching was ground into powder and placed in a tube furnace at 500°C with a heating rate of 5°C / min; it was calcined in an air atmosphere for 2h to obtain a microporous SiO2-modified MOF-derived cobalt-iron composite material CoFeCMs@mSiO2.

[0107] An application of a microporous SiO2-modified MOF-derived cobalt-iron composite material, the microporous SiO2-modified MOF-derived cobalt-iron composite material CoFeCMs@mSiO2 is applied to activate peroxymonosulfate to degrade ofloxacin.

[0108] The degradation method is as follows: 100 mL of 20 mg / L ofloxacin solution is put into a 1000 mL beaker, 0.04 g of microporous SiO2-modified MOF-derived cobalt-iron composite material CoFeCMs@mSiO2 and 0.03 g of peroxymonosulfate are added to the beaker, the beaker is placed on a shaker and shaken for 20 minutes, and the peroxymonosulfate is activated by the synergistic effect of the cobalt-iron bimetallic in the MOF-derived cobalt-iron composite material CoFeCMs@mSiO2 to degrade ofloxacin; 2-3 mL of the degraded solution is taken out with a syringe, the solution is filtered with a 0.22 μm polyethersulfone PES filter membrane and placed in a quartz cuvette, and the ofloxacin concentration is analyzed by UV-Vis at a wavelength of 294 nm, and the degradation rate of ofloxacin is 91.7%.

[0109] The XRD patterns of CoFeCMs@mSiO2 before and after catalytic reaction are shown in Fig.16 ,Depend on Fig.16 It can be seen that the characteristic peaks of CoFeCMs@mSiO2 did not change before and after the catalytic reaction, indicating that the structure of CoFeCMs@mSiO2 did not change, proving the stability of the catalyst.

[0110] The CoFeCMs@mSiO2 in the solution after the above degradation reaction was collected by centrifugation and used again for the experiment of degrading ofloxacin. The degradation experiment described in Example 1 was repeated 5 times. The recovered CoFeCMs@mSiO2 was washed and dried after each treatment of the pollutant. According to the test, the degradation rate of ofloxacin was 89.4% when degrading ofloxacin for the second time; the degradation rate of ofloxacin was 84.6% when degrading ofloxacin for the third time; the degradation rate of ofloxacin was 79.0% when degrading ofloxacin for the fourth time; and the degradation rate of ofloxacin was 69.1% when degrading ofloxacin for the fifth time.

[0111] The degradation data obtained from each degradation experiment were plotted with sampling time as the horizontal axis and the degradation rate of ofloxacin as the vertical axis. The degradation graph of CoFeCMs@mSiO2 for ofloxacin is shown in Fig.16 .Depend on Fig.16 It can be seen that CoFeCMs@mSiO2 can still quickly degrade ofloxacin in a short time within three cycle experiments, and keep the degradation rate of ofloxacin above 84%.

[0112] Fe-ZIF 67 with a molar ratio of Co to Fe of 1:1.5 was prepared by step 1, and Fe-ZIF 67 was calcined at 500°C to prepare CoFeCMs. The SEM image of the prepared CoFeCMs is shown in Figure 2 (c), it can be seen that the CoFeCMs structure collapses very seriously, and the cobalt-iron bimetallic oxides are deposited on the surface, making the surface rough.

[0113] The SEM image of CoFeCMs@mSiO2 prepared in Example 1 is shown in Figure 2 (b) By Figure 2 (b) It can be seen that the surface of Fe-ZIF 67 is coated with mesoporous SiO2 to form spherical nanoparticles with a particle size of about 300-600nm.

[0114] Example 2

[0115] The preparation method of the microporous SiO2 modified MOF-derived cobalt-iron composite material CoFeCMs@mSiO2 in this example is the same as that in Example 1.

[0116] Microporous SiO2-modified MOF-derived cobalt-iron composite CoFeCMs@mSiO2 was applied to activate peroxymonosulfate for the degradation of ofloxacin.

[0117] The degradation method is as follows: 100 mL of a 20 mg / L ofloxacin solution is put into a 1000 mL beaker, the beaker is placed on a shaker for shaking, 0.04 g of a microporous SiO2-modified MOF-derived cobalt-iron composite material CoFeCMs@mSiO2 and 0.04 g of peroxymonosulfate are added to the beaker, and the peroxymonosulfate is activated by the synergistic effect of the cobalt-iron bimetallic in the MOF-derived cobalt-iron composite material CoFeCMs@mSiO2 to degrade ofloxacin; the degradation time is 20 min, 2-3 mL of the solution in the degradation process is taken out with a syringe, the solution is filtered with a 0.22 μm polyethersulfone PES filter membrane and placed in a quartz cuvette, and the ofloxacin concentration is analyzed by UV-Vis at a wavelength of 294 nm, and the degradation rate of ofloxacin is 90.9%.

[0118] Example 3

[0119] The preparation method of the microporous SiO2 modified MOF-derived cobalt-iron composite material CoFeCMs@mSiO2 in this example is the same as that in Example 1.

[0120] Microporous SiO2-modified MOF-derived cobalt-iron composite CoFeCMs@mSiO2 was applied to activate peroxymonosulfate for the degradation of ofloxacin.

[0121] The degradation method is as follows: 100 mL of 20 mg / L ofloxacin solution is put into a 1000 mL beaker, the beaker is placed on a shaker for shaking, 0.05 g of microporous SiO2-modified MOF-derived cobalt-iron composite material CoFeCMs@mSiO2 and 0.03 g of peroxymonosulfate are added to the beaker, and the peroxymonosulfate is activated by the synergistic effect of the cobalt-iron bimetal in the MOF-derived cobalt-iron composite material CoFeCMs@mSiO2 to degrade ofloxacin; the degradation time is 20 min, 2-3 mL of the solution in the degradation process is taken out with a syringe, the solution is filtered with a 0.22 μm polyethersulfone PES filter membrane and placed in a quartz cuvette, and the ofloxacin concentration is analyzed by UV-Vis at a wavelength of 294 nm, and the degradation rate of ofloxacin is 91.6%.

[0122] Example 4

[0123] A method for preparing a microporous SiO2-modified MOF-derived cobalt-iron composite material comprises the following steps:

[0124] Step 1: Prepare the precursor Fe-ZIF 67 by co-precipitation method:

[0125] 10 mL of 1 mol / L NaOH and 10 mL of 3.36 mol / L 2-methylimidazole solution were mixed and stirred evenly, and the mixture was ultrasonicated for 10 min. The prepared solution was referred to as solution A.

[0126] Take 0.8 mL of 0.8 mol / L Co(NO3)2·6H2O and 9.6 mL of 0.1 mol / L FeCl3·6H2O solution, mix them evenly, dilute them to 12 mL with water, and use ultrasonic for 10 min as solution B.

[0127] Solution B was slowly added dropwise to solution A under stirring. After the addition was completed, stirring was continued at room temperature for 24 hours. The mixed solution was centrifuged to collect the solid matter at a centrifugal rate of 8000 rpm. The solid matter was then repeatedly washed with water and methanol alternately for several times and dried at 60° C. to obtain the precursor Fe-ZIF 67. The molar ratio of Co element to Fe element in the precursor Fe-ZIF 67 was 1:1.5.

[0128] Step 2: Preparation of Fe-ZIF 67@mSiO2:

[0129] The precursor Fe-ZIF 67 prepared in step 1 is dispersed in water to prepare a Fe-ZIF67 aqueous solution with a concentration of 1 mg / mL. 100 mL of the Fe-ZIF 67 aqueous solution is mixed with 20 mL of a 62.5 mg / mL hexadecyltrimethylammonium bromide ethanol solution and stirred for 1 h. The mixed solution is heated to 50°C, 0.5 mL of ammonia water is added, 583 mg of tetraethyl silicate is mixed with 10 mL of ethanol and then added dropwise to the mixed solution in 5 times, and stirred vigorously at 50°C for 6 h. After the reaction is completed, the solution is centrifuged at a centrifugal rate of 8000 rpm. The solid matter is collected, washed three times with ethanol, and dried at 60°C to obtain Fe-ZIF67@mSiO2.

[0130] Step 3: Preparation of Fe-ZIF 67@mSiO2 after removal of hexadecyltrimethylammonium bromide and water etching

[0131] The Fe-ZIF 67@mSiO2 prepared in step 2 is extracted with an ethanol solution of ammonium nitrate at 80°C to remove hexadecyltrimethylammonium bromide in the shell structure of Fe-ZIF 67@mSiO2;

[0132] After removing the hexadecyltrimethylammonium bromide, Fe-ZIF 67@mSiO2 was dispersed in water at a concentration of 2 mg / mL, and 70 mL of the dispersion was loaded into a 100 mL reactor and kept at 100 °C for 24 h.

[0133] The dispersion was centrifuged and the solid was collected, washed with ethanol, and dried at 60°C to obtain Fe-ZIF 67@mSiO2 after removal of hexadecyltrimethylammonium bromide and water etching;

[0134] Step 4: Calcination in air atmosphere to prepare CoFeCMs@mSiO2

[0135] The Fe-ZIF 67@mSiO2 prepared in step 3 after removal of hexadecyltrimethylammonium bromide and water etching was ground into powder and placed in a tube furnace at 600°C with a heating rate of 5°C / min; it was calcined for 2 hours in an air atmosphere to obtain a microporous SiO2-modified MOF-derived cobalt-iron composite material CoFeCMs@mSiO2.

[0136] An application of a microporous SiO2-modified MOF-derived cobalt-iron composite material, the microporous SiO2-modified MOF-derived cobalt-iron composite material CoFeCMs@mSiO2 is applied to activate peroxymonosulfate to degrade ofloxacin.

[0137] The degradation method is as follows: 100 mL of 20 mg / L ofloxacin solution is put into a 1000 mL beaker, 0.04 g of microporous SiO2-modified MOF-derived cobalt-iron composite material CoFeCMs@mSiO2 and 0.03 g of peroxymonosulfate are added to the beaker, the beaker is placed on a shaker and shaken for 20 minutes, and the peroxymonosulfate is activated by the synergistic effect of the cobalt-iron bimetallic in the MOF-derived cobalt-iron composite material CoFeCMs@mSiO2 to degrade ofloxacin; 2-3 mL of the degraded solution is taken out with a syringe, the solution is filtered with a 0.22 μm polyethersulfone PES filter membrane and placed in a quartz cuvette, and the ofloxacin concentration is analyzed by UV-Vis at a wavelength of 294 nm, and the degradation rate of ofloxacin is 90.4%.

[0138] Example 5

[0139] The preparation method of the microporous SiO2 modified MOF-derived cobalt-iron composite material in this example is the same as that in Example 1.

[0140] An application of a microporous SiO2-modified MOF-derived cobalt-iron composite material, the microporous SiO2-modified MOF-derived cobalt-iron composite material CoFeCMs@mSiO2 is applied to activate peroxymonosulfate to degrade ofloxacin.

[0141] The degradation method is as follows: 100 mL of a 30 mg / L ofloxacin solution is put into a 1000 mL beaker, the beaker is placed on a shaker for shaking, 0.04 g of a microporous SiO2-modified MOF-derived cobalt-iron composite material CoFeCMs@mSiO2 and 0.03 g of peroxymonosulfate are added to the beaker, and the peroxymonosulfate is activated by the synergistic effect of the cobalt-iron bimetallic in the MOF-derived cobalt-iron composite material CoFeCMs@mSiO2 to degrade ofloxacin; the degradation time is 20 min, 2-3 mL of the solution in the degradation process is taken out with a syringe, the solution is filtered with a 0.22 μm polyethersulfone PES filter membrane and placed in a quartz cuvette, and the ofloxacin concentration is analyzed by UV-Vis at a wavelength of 294 nm, and the degradation rate of ofloxacin is 88.9%.

[0142] The above are only preferred embodiments of the present invention. It should be noted that for those skilled in the art, other equivalent variations and improvements can be made under the technical enlightenment provided by the present invention, which should also be considered as the protection scope of the present invention.

Claims

1. A method for preparing a microporous SiO2-modified MOF-derived cobalt-iron composite material, characterized in that: The following steps are involved: Step 1: Prepare the precursor Fe-ZIF 67 by co-precipitation method: 10 mL of 1 mol / L NaOH and 10 mL of 3.36 mol / L 2-methylimidazole solution were mixed and stirred evenly, and the mixture was ultrasonicated for 10 min. The prepared solution was referred to as solution A. Take 0.8 mL of 0.8 mol / L Co(NO3)2·6H2O and 9.6 mL of 0.1 mol / L FeCl3·6H2O solution, mix them evenly, dilute them to 12 mL with water, and use ultrasonic for 10 min as solution B. Under stirring conditions, solution B was slowly added dropwise to solution A. After the addition was completed, stirring was continued at room temperature for 24 hours. The mixed solution was centrifuged to collect the solid matter. The solid matter was then repeatedly washed with water and methanol alternately for several times and dried at 60° C. to obtain the precursor Fe-ZIF 67. The molar ratio of Co element to Fe element in the precursor Fe-ZIF 67 was 1:1.

5. Step 2: Preparation of Fe-ZIF 67@mSiO2: The precursor Fe-ZIF 67 prepared in step 1 is dispersed in water to prepare a Fe-ZIF 67 aqueous solution with a concentration of 1 mg / mL. 100 mL of the Fe-ZIF 67 aqueous solution is mixed with 20 mL of a 62.5 mg / mL hexadecyltrimethylammonium bromide ethanol solution and stirred for 1 h. The mixed solution is heated to 50°C, 0.5 mL of ammonia water is added, 583 mg of tetraethyl silicate is mixed with 10 mL of ethanol and then added dropwise to the mixed solution several times, and stirred vigorously at 50°C for 6 h. After the reaction is completed, the solution is centrifuged, the solid is collected, the solid is washed three times with ethanol, and dried at 60°C to obtain Fe-ZIF 67@mSiO2. Step 3: Preparation of Fe-ZIF 67@mSiO2 after removal of hexadecyltrimethylammonium bromide and water etching: Extract the Fe-ZIF 67@mSiO2 prepared in step 2 with an ethanol solution of ammonium nitrate at 80°C to remove hexadecyltrimethylammonium bromide in the shell structure of Fe-ZIF 67@mSiO2; After removing the hexadecyltrimethylammonium bromide, Fe-ZIF 67@mSiO2 was dispersed in water at a concentration of 2 mg / mL, and 70 mL of the dispersion was loaded into a 100 mL reactor and kept at 100 °C for 24 h. The dispersion was centrifuged and the solid was collected, washed with ethanol, and dried at 60°C to obtain Fe-ZIF 67@mSiO2 after removal of hexadecyltrimethylammonium bromide and water etching; Step 4: Calcination in air atmosphere to prepare CoFeCMs@mSiO2 The Fe-ZIF 67@mSiO2 prepared in step 3 after removal of hexadecyltrimethylammonium bromide and water etching was ground into powder, placed in a tube furnace at 300-700°C, and calcined for 2 hours in an air atmosphere to obtain a microporous SiO2-modified MOF-derived cobalt-iron composite material CoFeCMs@mSiO2.

2. The method for preparing the microporous SiO2-modified MOF-derived cobalt-iron composite material according to claim 1, characterized in that: In the step 2, tetraethyl silicate is added dropwise to the mixed solution in 5 portions.

3. The method for preparing the microporous SiO2-modified MOF-derived cobalt-iron composite material according to claim 1, characterized in that: The centrifugal speed of the solution in step 1 and step 2 is 8000 rpm.

4. The method for preparing the microporous SiO2-modified MOF-derived cobalt-iron composite material according to claim 1, characterized in that: The heating rate of the tubular furnace in step 4 is 5°C / min.

5. Application of a microporous SiO2-modified MOF-derived cobalt-iron composite material, characterized in that: Microporous SiO2-modified MOF-derived cobalt-iron composite CoFeCMs@mSiO2 was applied to activate peroxymonosulfate for the degradation of ofloxacin.

6. The use of the microporous SiO2-modified MOF-derived cobalt-iron composite material according to claim 5, characterized in that: The degradation method is as follows: 100 mL of a 10-30 mg / L ofloxacin solution is put into a 1000 mL beaker, the beaker is placed on a shaker for shaking, 0.02-0.06 g of a microporous SiO2-modified MOF-derived cobalt-iron composite material CoFeCMs@mSiO2 and 0.01-0.05 g of peroxymonosulfate are added to the beaker, and the peroxymonosulfate is activated by the synergistic effect of the cobalt-iron bimetal in the MOF-derived cobalt-iron composite material CoFeCMs@mSiO2 to degrade ofloxacin; the degradation time is 20 min, 2-3 mL of the solution in the degradation process is taken out with a syringe, the solution is filtered with a 0.22 μm polyethersulfone PES filter membrane and placed in a quartz cuvette, and the ofloxacin concentration is analyzed by UV-Vis at a wavelength of 294 nm.

Citation Information

Patent Citations

  • Cobalt-iron bimetal in-situ doped MCM-41 catalyst, and preparation method and application thereof

    CN109999890A

  • High-dispersion ferrocobalt bimetallic catalyst as well as preparation method and application thereof

    CN113198517A

  • Preparation of biochar-modified ferrocobalt bimetallic composite catalyst and application of biochar-modified ferrocobalt bimetallic composite catalyst in catalytic degradation of tetracycline

    CN114425340A

  • MOFs-derived Fe-N / C catalyst containing defect Fe-Nx as well as preparation method and application of MOFs-derived Fe-N / C catalyst

    CN115041211A

  • Core-shell structure ferrocobalt bimetallic catalyst and preparation method and application thereof

    CN115646493A