Preparation method and application of hydrodeoxygenation difunctional NiNb-based catalyst
The Ni/Nb@Si catalyst prepared by the sol-gel method solves the problem of insufficient deoxygenation capacity of existing catalysts in the hydrodeoxygenation reaction of lignin, and realizes the efficient conversion of lignin derivatives into cycloalkanes, which has good economic and environmental benefits.
Patent Information
- Application Number
- CN202411060982.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-05
AI Technical Summary
Existing Ni-based catalysts have insufficient deoxygenation capacity in the hydrodeoxygenation reaction of lignin, and traditional preparation methods result in uneven dispersion of the active phase and high cost, making it difficult to efficiently convert lignin derivatives into cycloalkanes under mild conditions.
Ni/Nb@Si catalysts were formed by using niobium oxide-doped silica as a support via sol-gel method and loading nickel precursors via equal-volume impregnation method. The preparation process was optimized to improve specific surface area and pore volume, thereby enhancing catalytic activity.
It significantly improves the conversion rate of lignin derivatives and the selectivity of cycloalkanes under mild conditions, while reducing catalyst costs, demonstrating good economic and environmental benefits.
Smart Images

Figure CN118988336A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of hydrodeoxygenation of lignin derivatives, and in particular to a method for preparing a nickel-loaded catalyst with niobium-doped silicon dioxide as a carrier, and the field of preparing cycloalkane fuel by hydrodeoxygenation of lignin-derived model compounds. Background Art
[0002] Lignin is a polymer material with huge reserves and stable production. It is widely present in the cells of lignified plants and regenerates at a rate of about 50 billion tons per year, with great potential for utilization. The global pulp and paper industry alone can obtain about 70 million tons of lignin byproducts from plants every year, but more than 95% of the lignin is discharged into rivers in the form of "black liquor" or burned after concentration, and the utilization rate is very low. The monomers and dimers derived from lignin are mainly phenols and ethers. They can be hydrodeoxygenated (HDO) to obtain hydrocarbon substances with a carbon number distribution between 6 and 10, which is basically consistent with the carbon number distribution of commercial gasoline components and is an ideal green biofuel (CN 110066677A). Therefore, it is particularly important to find a catalyst that is simple, easy to obtain and efficient in depolymerizing lignin to obtain liquid fuel for the efficient utilization of lignin.
[0003] From the perspective of catalyst composition, HDO of phenolic compounds requires a bifunctional catalyst involving hydrogenation on the metal site and dehydration / deoxygenation on the support.
[0004] Non-precious metals have significant economic advantages over precious metals and have received widespread attention. Although non-precious metals have shown good hydrogenation or oxygen affinity, single non-precious metal system catalysts are still slightly inferior to precious metals. Compared with other transition metals, Ni has a wider d electron band and higher energy density. These unique properties can greatly improve the adsorption and activation ability of hydrogen molecules, thereby providing more active hydrogen species for hydrogenation reactions (Green Chemistry, 2020, 22 (23), 8140-8168; Green Chemistry, 2016, 18, 5845-5858). Among several transition metal catalysts such as Ni, Fe, Cu, Zn, and Sn, Ni-based catalysts show the best activity and product selectivity for the value-added production of renewable chemicals and fuels from lignin. Most of the existing Ni-based catalysts can achieve a conversion rate of more than 85% for the typical lignin derivative guaiacol, but the average selectivity of the main product cyclohexane is less than 75%, and there are also a variety of oxygen-containing by-products such as phenol and cyclohexanol. Because the fragmentation dissociation energy of hydroxyl groups is very high, it is generally believed that 300°C is necessary to obtain high HDO efficiency in non-precious metal systems. Some reaction temperatures even require up to 400°C, indicating that deoxygenation is the technical key to this type of reaction. Usually, researchers will prepare bimetallic or bifunctional catalyst systems containing non-precious metals to maximize their performance advantages. Therefore, it is necessary to introduce a second metal or other additives for modification so that the deoxygenation effect can be better exerted, and it is necessary to develop catalysts with excellent performance under milder reaction conditions.
[0005] As a new type of catalytic material, niobium compounds have played a significant role in promoting many types of catalytic reactions such as hydrodeoxygenation, hydrodesulfurization, ammoxidation and solid acid reaction, and can be used as an additive or carrier to enhance the reaction activity. Patent CN114870853B combines the template method with the impregnation method to introduce Nb metal modification during the shell formation process to form a functional Co@Nb-WO x -MSiO 2 YSNSs catalysts were used for hydrogenation of guaiacol to cyclohexanol, and the additives Nb and WO were found xThe introduction of niobium improves the catalytic activity of metal Co, the dispersion of metal and the acid sites of the catalyst. When single niobium pentoxide is used as a carrier, there are problems such as too small specific surface area and too high acidity (Catal. Today, 2017, 285, 211-225). Doping niobium species into the network of other oxides helps to adjust the acidity, thermal stability and specific surface area of the original carrier, and can further improve its performance by introducing lattice defects. Fernandes et al. (JTAC, 2017, 131 (1), 691-5) doped niobium into MCM-41 nanostructured materials and verified the changes in the surface properties and acidic functions of the materials. Patent CN 107812516 B provides a preparation method for cerium dioxide doped with niobium pentoxide, its products and applications. When it is loaded with precious metals, it exhibits good benzene combustion performance, but polyvinyl alcohol needs to be added as a solubilizer during the preparation process to avoid precipitation of cerium ions due to the addition of oxalate. Patent CN 105939775 A uses an impregnation method to prepare a cerium oxide catalyst doped with niobium oxide or tantalum oxide, which is used in a selective catalytic reduction reaction. However, due to the low solubility of niobium salts, the impregnation method often has the disadvantage of uneven particle distribution when preparing niobium-doped compounds. Currently, the two technologies closest to the present invention are as follows: Patent CN 113680347A uses cheap SiO 2 The carrier was modified by adding soluble precursors of Ce, Ta and Nb to prepare catalysts for oil hydrodesulfurization and regulation of aromatic ring saturation; Patent CN 113441139A prepared Pd, Pt and Ni-loaded Nb 2 O 5 -SiO 2 Catalyst for catalyzing the hydrodeoxygenation reaction of the condensation products of sugar platform compounds to prepare liquid alkanes. However, during the impregnation process, the carrier needs to be immersed in the impregnation solution for a long time (CN 113441139A), and the excessively high drying temperature leads to uneven dispersion of the active phase, and also causes a loss of 1-3wt% of the active metal component (CN 113680347A), resulting in a large difference between the actual metal loading and the theoretical loading, and the amount of precursor is difficult to control, and the preparation cost of the catalyst is increased. In addition, the specific surface area and pore volume of the carrier are not increased enough during the doping process, and the overall catalytic performance needs to be improved.
[0006] Most of the methods used to dope transition metal oxides are traditional methods. For example, the impregnation method will lead to uneven dispersion of the active phase and loss of active metals; the coprecipitation method requires long-term stirring, and will introduce alkaline substances, and also requires filtration and washing; the hydrothermal method often requires high temperature and high pressure, and the preparation time is also relatively long. The sol-gel method has the advantages of short preparation time, simple operation, no need for filtration and washing, and less loss of catalyst components. However, the sol-gel method still needs to be optimized, for example, by controlling the heating rate to adjust the crystallization, and the temperature and time of cross-linking and drying will affect the grain growth and further affect the microscopic morphology of the product. Summary of the invention
[0007] The purpose of the present invention is to provide a preparation method and application of a hydrogenation and deoxygenation bifunctional NiNb-based catalyst in view of the shortcomings of current catalysts. The method uses an optimized sol-gel method to prepare silicon dioxide doped with niobium species as a carrier, and uses an equal amount of impregnation method to load a nickel-containing precursor on a composite carrier doped with a niobium additive; only a nickel source, a niobium source, a complexing agent and a silicon source are required, and other initiators, promoters and solubilizers are not required, which can reduce the interference of impurities, reduce costs and simplify the process; the use of a complexing agent can help form a metal ion complex, control the concentration of metal ions, and also help to adjust the pH value of the reaction system, thereby promoting the formation of gel and improving the quality of gel, and increasing the specific surface area and pore volume of the catalyst. The content of oxygen vacancies in the doped catalyst obtained by the present invention is significantly improved, which greatly promotes the deoxygenation effect, effectively makes up for the problem of insufficient deoxygenation capacity of existing catalysts mentioned in the background technology, and has very strong advantages and significant applicability in the lignin-derived phenol HDO system.
[0008] The technical solution of the present invention is:
[0009] A method for preparing a hydrodeoxygenation bifunctional NiNb-based catalyst, the method comprising the following steps:
[0010] (1) adding a silicon source to deionized water, stirring magnetically for 5-30 minutes, then adding a complexing agent, and continuing to stir magnetically for 5-30 minutes to obtain a solution A;
[0011] The mass ratio of the added components is silicon source: complexing agent: deionized water = 1:0.1-0.5:4-12;
[0012] (2) adding the niobium source to the solution A obtained in step (1) under stirring, and continuing magnetic stirring for 2-8 hours to obtain a homogeneous hydrogel prepolymer solution B;
[0013] Wherein, the mass ratio is niobium source:silicon source=1:1-21;
[0014] (3) drying the hydrogel prepolymer solution B obtained in step (2) in stages, wherein the first stage is drying at a constant temperature of 40-60° C. for 4-6 hours, taking out and grinding; and then drying at a constant temperature of 40-60° C. for another 4-6 hours to obtain a dry solid;
[0015] (4) calcining the dried solid obtained in step (3) in a muffle furnace at 400-600° C. for 3-5 h at a heating rate of 1-5° C. / min to obtain a yNb@Si sample, i.e., a silica composite oxide support doped with niobium species;
[0016] Wherein, y represents the doping amount of niobium species in the carrier, which is 4-45wt%;
[0017] (5) measuring the saturated water absorption of the composite oxide support obtained in step (4), and then dripping the nickel source solution onto the support by an equal amount impregnation method;
[0018] (6) drying the sample obtained in step (5) at 30-40° C. for 10-12 h;
[0019] (7) calcining the dried sample in step (6) at 400-600° C. in a muffle furnace for 3-5 h;
[0020] (8) The sample calcined in step (7) is reduced in a tubular furnace in a flowing hydrogen atmosphere at 400-600° C. for 3-5 h to obtain an xNi / yNb@Si catalyst, i.e., a hydrogenation and deoxygenation bifunctional NiNb-based catalyst.
[0021] Optionally, the silicon source in step (1) is one or more of ethyl orthosilicate, methyl orthosilicate, butyl orthosilicate, isopropyl orthosilicate and alkyl alkoxy silane;
[0022] Optionally, the complexing agent in step (1) includes one or more of citric acid, tartaric acid, ethylenediaminetetraacetic acid, malic acid, glycolic acid, and succinic acid;
[0023] Optionally, the niobium source in step (2) includes one or more of niobium oxalate, niobium pentachloride, niobium ethoxide, niobium acetate, ammonium niobate oxalate hydrate or niobium hydroxide;
[0024] Optionally, the nickel source in step (5) includes one or more of nickel nitrate, nickel chloride, nickel carbonate and nickel oxalate; and the concentration of the nickel source solution is 1-4 mol / L.
[0025] Furthermore, the hydrodeoxygenation bifunctional NiNb-based catalyst is characterized in that, during the catalyst formation process, due to the strong metal-carrier interaction, nickel niobate is formed on the nickel-niobium interface and niobium oxide of a special crystalline phase is formed in the carrier, which can serve as acidic sites and are beneficial to the removal of oxygen-containing functional groups.
[0026] In terms of mass percentage, the doping amount of the Nb additive in the composite carrier is 4-45wt%, and the content of the Ni active component on the catalyst is 1-10wt%.
[0027] The hydrodeoxygenation bifunctional NiNb-based catalyst prepared by the method is used as a catalyst in the process of preparing cycloalkane fuel by hydrodeoxygenation reaction of lignin derivatives.
[0028] The specific steps are as follows:
[0029] A lignin derivative, n-dodecane and a hydrodeoxygenation bifunctional NiNb-based catalyst are added to a reaction kettle, which is sealed and replaced with 0.5-2 MPa argon gas in the kettle, and reacted for 0.5-10 h under a hydrogen pressure of 3-7 MPa, 200-260° C. and stirring to obtain cycloalkanes;
[0030] Wherein, the mass ratio of feed is catalyst: reactant: solvent = 1:5-100:490-2400; preferably, the mass ratio of catalyst to reactant is 1:10;
[0031] The lignin derivatives are common and representative lignin-derived phenolic substances, including one or more of phenol, m-cresol, p-cresol, guaiacol, 2-methoxy-4-propylphenol, eugenol and 2,6-dimethoxyphenol, and one or more of lignin-derived dimer substances containing β-O-4, α-O-4, and 4-O-5 bonds.
[0032] Preferably, the reaction temperature is 250° C., the reaction pressure is 5 MPa, the reaction time is 2 h, and the metal loading in the xNi / yNb@Si catalyst is 10 wt % Ni and 20 wt % Nb.
[0033] The cycloalkane is one or more of cyclohexane, methylcyclohexane, ethylcyclohexane, propylcyclohexane, methylcyclopentane and methylcyclobutane.
[0034] The essential features of the present invention are:
[0035] The present invention adopts the sol-gel method to dope niobium oxide into SiO 2 The network was impregnated with nickel precursors in equal amounts to prepare a stable Ni / Nb@Si catalytic system, which was applied to the hydrodeoxygenation of lignin-derived phenolic compounds to prepare cycloalkane fuels. Among them, when the niobium source is introduced during the hydrolysis of the silicon source into gel, Nb will enter the SiO 2In the framework, the formation of Nb-O bonds will partially replace Si-O bonds, causing the unit cell parameters and unit cell stacking mode of the composite carrier to change accordingly, resulting in a significant increase in the specific surface area of the carrier material; at the same time, due to the different atomic sizes of niobium and silicon, when the grains grow, it is easy to deform the crystal structure and introduce lattice defects, thereby changing the acidity of the carrier and generating a large number of oxygen vacancies; further, when the Nb content is too high, it is difficult for Nb to completely enter the SiO 2 Skeleton, will generate independent Nb 2 O 5 Crystalline phase, so that the specific surface area and oxygen vacancies will be reduced to a certain extent; preferably, the niobium doping amount is 5-20wt%.
[0036] Compared with the prior art, the present invention has the following beneficial effects:
[0037] (1) The composite oxide carrier is obtained by the sol-gel method in the present invention, which makes up for the shortcomings of a single carrier, increases the specific surface area of the catalyst, improves the dispersibility of the active metal nickel, and the synergistic effect of the metal site and the carrier improves the catalyst performance. From the change in specific surface area, Nb 2 O 5 6m 2 / g,SiO 2 636m 2 / g, the doped 5Nb@Si increased to 811m 2 / g, compared with Nb in patent CN 113441139 A 2 O 5 -SiO 2 The specific surface area of the composite oxide is increased by 311-511m 2 / g. From the reaction results of Examples 6-12, when only silicon dioxide or niobium pentoxide is used as a carrier to load Ni, the selectivity of catalyzing the hydrodeoxygenation of guaiacol to obtain cyclohexane is less than 20%; while when Ni is loaded on the niobium silicon composite carrier, the selectivity of cyclohexane is greater than 55%, which is significantly improved, and the highest can even reach 94.37%, and the reactant conversion rate can reach 100%.
[0038] (2) The catalyst of the present invention can achieve efficient conversion of lignin derivatives under relatively mild conditions and generate cycloalkanes with high selectivity. The apparent activation energy of the HDO reaction on the 10Ni / 20Nb@Si catalyst was calculated to be 54.23 kJ·mol -1 , which is better than the best result reported so far on non-precious metal catalysts, namely NiCo / SiO 2 -ZrO 2 55.9 kJ·mol on catalyst -1(Fuel, 2022, 308, 122034). The obtained catalyst has a significant effect on the hydrogenation and deoxygenation of common lignin derivatives, has strong universality, and has good application prospects.
[0039] (3) In the present invention, the catalyst preparation cycle is short and the process flow is simple; the materials used for the reaction raw materials and catalysts are inexpensive, which can significantly reduce costs; transition metals such as nickel (the price is 133.375 yuan / kg as of July 12, 2024) and niobium (the price is 670 yuan / kg as of July 12, 2024) are more economical than precious metals such as platinum (the price is 212,060 yuan / kg as of July 12, 2024) and palladium (the price is 262,000 yuan / kg as of July 12, 2024). In addition, the impact of nickel metal on the global warming trend is estimated to be about 6.5 kg CO 2 Equivalent / kg, while platinum metal is 12,500kg CO 2 Equivalent / kg, so the components and raw materials selected in the present invention are more economical and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 The different catalysts obtained in Examples 1-5 and Comparative Example 1 were 2 XRD spectrum after reduction under atmosphere.
[0041] Figure 2 N of different catalysts obtained in Examples 1-5 and Comparative Example 1 2 Physical adsorption and desorption characterization results; among them, Figure 2 (a) is N 2 Physical adsorption-desorption isotherms; Figure 2 (b) is the pore size distribution diagram.
[0042] Figure 3 The different carriers and catalysts obtained in Examples 2-4 and Comparative Example 1 Acid and Lewis acid characteristic peaks.
[0043] Figure 4 The O1s and Ni2p of the catalysts obtained in Examples 2-4 and Comparative Examples 1-2 3 / 2 and Nb3d XPS spectra, where O α Represents the characteristic peaks related to lattice oxygen, O β Represents the characteristic peaks of vacant oxygen associated with oxygen defects. DETAILED DESCRIPTION
[0044] The present invention is described below by specific embodiments. Unless otherwise specified, the technical means used in the present invention are methods known to those skilled in the art. In addition, the embodiments should be understood as illustrative, rather than limiting the scope of the present invention, and the essence and scope of the present invention are limited only by the claims. The experimental methods without specifying specific conditions in the examples are usually based on conventional conditions and the conditions described in the manual, or the general equipment, materials, reagents, etc. used according to the conditions recommended by the manufacturer, and if not otherwise specified, can all be obtained from commercial sources. The present invention is further described below in conjunction with specific examples.
[0045] Preparation method of catalyst:
[0046] Example 1
[0047] 12.38g of tetraethyl orthosilicate (TEOS) of silicon source was added to 49.54g of deionized water, and magnetic stirring was continued for 10min. Then, 3.84g of citric acid (CA) of complexing agent was added, and magnetic stirring was continued for 10min. Then, 0.7604g of niobium oxalate of niobium source was added to the solution, and magnetic stirring was continued for 6h to obtain a homogeneous hydrogel prepolymer solution. The obtained hydrogel prepolymer solution was segmented and dried. In the first stage, it was dried at a constant temperature of 50℃ for 4h to make the hydrogel cross-linked and formed until there was no liquid in the container. After the prepolymer solution became a jelly-like solid, it was taken out and ground into small particles with a mortar; in the second stage, it was continued to be dried at a constant temperature of 50℃ for 5h to remove the water and all other volatiles inside. Then the dried solid was calcined at 600℃ (heating rate 2℃ / min) for 3h in a muffle furnace to obtain a composite oxide carrier with a Nb doping amount of about 5wt%, which was recorded as 5Nb@Si sample. According to the saturated water absorption of 5Nb@Si carrier, 2.2015 g of Ni(NO 3 ) 2 6H 2 O was dissolved in 2.80g of deionized water, ultrasonically dispersed for 30min to obtain a nickel source solution, and the nickel source solution was added dropwise to 4.0g of 5Nb@Si carrier by equal volume impregnation method. Then it was dried at 30℃ for 12h, calcined at 500℃ (heating rate 5℃ / min) for 3h, and reduced at 500℃ (heating rate 5℃ / min) for 3h in a tubular furnace in a flowing hydrogen atmosphere of 80mL / min to obtain a 10Ni / 5Nb@Si catalyst (10Ni represents that the active metal Ni loaded accounts for 10wt% of the total mass of the catalyst, and 5Nb represents that the doping amount of niobium species in the carrier is 5wt%).
[0048] Example 2
[0049] 12.38g of tetraethyl orthosilicate (TEOS) of silicon source was added to 49.54g of deionized water, and magnetic stirring was continued for 10min. Then, 3.84g of citric acid (CA) of complexing agent was added, and magnetic stirring was continued for 10min. Then, 1.6053g of niobium oxalate of niobium source was added to the solution, and magnetic stirring was continued for 6h to obtain a homogeneous hydrogel prepolymer solution. The obtained hydrogel prepolymer solution was subjected to the same segmented drying treatment as in Example 1, and then the dried solid was calcined at 600℃ (heating rate 2℃ / min) in a muffle furnace for 3h to obtain a composite carrier with a Nb doping amount of about 10wt%, which was recorded as 10Nb@Si sample. The loading method of nickel source was the same as in Example 1 to obtain 10Ni / 10Nb@Si catalyst.
[0050] Example 3
[0051] 12.38g of tetraethyl orthosilicate (TEOS) of silicon source was added to 49.54g of deionized water, and magnetic stirring was performed for 10min. Then, 3.84g of citric acid (CA) of complexing agent was added, and magnetic stirring was continued for 10min. Then, 3.6119g of niobium oxalate of niobium source was added to the solution, and magnetic stirring was continued for 6h to obtain a homogeneous hydrogel prepolymer solution. The obtained hydrogel prepolymer solution was subjected to the same segmented drying treatment as in Example 1, and then the dried solid was calcined at 600°C (heating rate 2°C / min) in a muffle furnace for 3h to obtain a composite carrier with a Nb doping amount of about 5wt%, which was recorded as a 20Nb@Si sample. The loading method of the nickel source was the same as in Example 1, and a 10Ni / 20Nb@Si catalyst was obtained.
[0052] Example 4
[0053] 12.38g of tetraethyl orthosilicate (TEOS) of silicon source was added to 49.54g of deionized water, and magnetic stirring was performed for 10min. Then, 3.84g of citric acid (CA) of complexing agent was added, and magnetic stirring was continued for 10min. Then, 6.1919g of niobium oxalate of niobium source was added to the solution, and magnetic stirring was continued for 6h to obtain a homogeneous hydrogel prepolymer solution. The obtained hydrogel prepolymer solution was subjected to the same segmented drying treatment as in Example 1, and then the dried solid was calcined at 600°C (heating rate 2°C / min) in a muffle furnace for 3h to obtain a composite carrier with a Nb doping amount of about 5wt%, which was recorded as a 30Nb@Si sample. The loading method of the nickel source was the same as in Example 1, and a 10Ni / 30Nb@Si catalyst was obtained.
[0054] Example 5
[0055] 12.38g of tetraethyl orthosilicate (TEOS) of silicon source was added to 49.54g of deionized water, and magnetic stirring was performed for 10min. Then, 3.84g of citric acid (CA) of complexing agent was added, and magnetic stirring was continued for 10min. Then, 9.6317g of niobium oxalate of niobium source was added to the solution, and magnetic stirring was continued for 6h to obtain a homogeneous hydrogel prepolymer solution. The obtained hydrogel prepolymer solution was subjected to the same segmented drying treatment as in Example 1, and then the dried solid was calcined at 600°C (heating rate 2°C / min) in a muffle furnace for 3h to obtain a composite carrier with a Nb doping amount of about 5wt%, which was recorded as a 40Nb@Si sample. The loading method of the nickel source was the same as in Example 1, and a 10Ni / 40Nb@Si catalyst was obtained.
[0056] Comparative Example 1
[0057] The same sol-gel method as in Example 1 was used to synthesize SiO 2 , and then loaded with 10wt% Ni to obtain 10Ni / SiO 2 catalyst.
[0058] Comparative Example 2
[0059] The same sol-gel method as in Example 1 was used to synthesize Nb 2 O 5 , and then loaded with 10wt% Ni to obtain 10Ni / Nb 2 O 5 catalyst.
[0060] Depend on Figure 1 From the XRD results, it can be seen that with the increase of Nb content, the diffraction peak of amorphous TT-niobium pentoxide appears, and the diffraction peaks at 2θ of 44.5, 51.8 and 76.4° belong to Ni (111), (200) and (220) planes, respectively (PDF#87-0712), indicating the formation of FCC (face-centered cubic) Ni phase.
[0061] from Figure 2 The results show that the prepared catalysts have similar pore size distribution and pore structure, and the most probable pore size is 3-4 nm. 2 O 5 The specific surface area is only 6m 2 / g, but after doping niobium oxide into the silicon oxide network, the specific surface area of the obtained 5Nb@Si carrier increased to 811m 2 / g, when the Nb doping amount is too high, Nb is difficult to completely enter SiO 2 Skeleton, will generate independent Nb 2 O 5 Crystalline phase, the specific surface area of 40Nb@Si is reduced to 226m2 / g, so the niobium doping amount has a key influence on the structure.
[0062] Comparative Example 3
[0063] The other steps are the same as those in Example 1, except that the obtained hydrogel prepolymer solution is not subjected to segmented drying, but is directly subjected to continuous constant temperature drying at 50° C. for 10 h. After continuous drying, the final dried solid obtained will become a large hard solid in the shape of broken glass, which is difficult to grind into small particles or powder, resulting in poor subsequent calcination effect, incomplete calcination, and difficulty in converting and releasing organic matter inside the large solid, which has an adverse effect on the catalyst performance.
[0064] The inventors have explored a method of segmented drying through experiments. The first stage of drying causes a chemical reaction inside the catalyst to form doping and cross-linking between different species. The catalyst will gradually transform from a solution to a sol and then to a gel. When there is no liquid in the container and the prepolymer becomes a molten jelly-like solid, it is taken out of the oven and ground in a mortar into small particles. The second stage of drying is then carried out until it is completely dried (4-6 hours), thereby achieving a more uniform and complete roasting.
[0065] Table 1 Specific surface area and pore structure information of different samples
[0066]
[0067] exist Figure 3 In the 1449, 1490 and 1616 cm -1 The peak at 1540 cm -1 The peak at corresponds to pyridine at The adsorption on the acid sites confirmed that Lewis acids dominated the acid sites on the catalyst surface, which was mainly attributed to the presence of coordination-unsaturated Ni and Nb cations.
[0068] exist Figure 4 The O1s spectrum can be decomposed into a characteristic peak at 530.4 eV related to the lattice oxygen in the sample (O α ) and the characteristic peak of vacancy oxygen related to oxygen defects at 532.5 eV (O β ). In 10Ni / SiO 2 and 10Ni / Nb 2 O 5 In the catalyst, O α >O β In the Ni / Nb@Si sample, O α <O β , indicating that there are more oxygen vacancies in the sample after niobium doping.
[0069] The catalyst obtained by the present invention comprises an active component, a metal additive and a carrier, and can realize the dual functions of hydrogenation and deoxygenation; wherein the nickel species is the hydrogenation active component, and the doped niobium species is the deoxygenation active component. The catalyst can be applied to the reaction of preparing cycloalkanes by hydrogenation and deoxygenation of lignin derivatives, and the following are specific examples.
[0070] Example 6
[0071] Add materials into a 100 mL high pressure mechanical stirring kettle, the mass ratio of the materials is catalyst: reactant: solvent = 1:10:490. In this embodiment, the catalyst used is the catalyst 10Ni / SiO obtained in Comparative Example 1. 2 , mass is 0.05g, the reactant is guaiacol, and the solvent is n-dodecane. Assemble the reactor and check the airtightness of the device, then fill argon from the reaction inlet, and replace the gas in the reactor several times until the air content is negligible. Turn on the condensing water, turn on the mechanical stirring to a certain speed (generally 800r / min), set the heating program and start heating. Using 5MPa hydrogen as the hydrogen source, react at a temperature of 250℃ for 2h, the conversion rate and selectivity data of the relevant species are calculated and shown in Table 2.
[0072] Example 7
[0073] Feed materials into a 100 mL high pressure mechanical stirring kettle, the mass ratio of the materials is catalyst: reactant: solvent = 1:10:490. In this embodiment, the catalyst 10Ni / 5Nb@Si obtained in Example 1 is selected, the mass is 0.05 g, the reactant is guaiacol, and the solvent is n-dodecane. The pre-reaction treatment and reaction conditions are the same as in Example 6, and the conversion rate and selectivity data of the relevant species are calculated and shown in Table 2.
[0074] Example 8
[0075] Feed materials into a 100 mL high pressure mechanical stirring kettle, the mass ratio of the materials is catalyst: reactant: solvent = 1:10:490. In this embodiment, the catalyst 10Ni / 10Nb@Si obtained in Example 2 is selected, the mass is 0.05 g, the reactant is guaiacol, and the solvent is n-dodecane. The pre-reaction treatment and reaction conditions are the same as in Example 6, and the conversion rate and selectivity data of the relevant species are calculated and shown in Table 2.
[0076] Example 9
[0077] Feed materials into a 100 mL high pressure mechanical stirring kettle, the mass ratio of the materials is catalyst: reactant: solvent = 1:10:490. In this embodiment, the catalyst 10Ni / 20Nb@Si obtained in Example 3 is selected, the mass is 0.05 g, the reactant is guaiacol, and the solvent is n-dodecane. The pre-reaction treatment and reaction conditions are the same as in Example 6, and the conversion rate and selectivity data of the relevant species are calculated and shown in Table 2.
[0078] Example 10
[0079] Feed materials into a 100 mL high pressure mechanical stirring kettle, the mass ratio of the feed materials is catalyst: reactant: solvent = 1:10:490. In this embodiment, the catalyst 10Ni / 30Nb@Si obtained in Example 4 is selected, the mass is 0.05 g, the reactant is guaiacol, and the solvent is n-dodecane. The pre-reaction treatment and reaction conditions are the same as in Example 6, and the conversion rate and selectivity data of the relevant species are calculated and shown in Table 2.
[0080] Embodiment 11
[0081] Feed materials into a 100 mL high pressure mechanical stirring kettle, the mass ratio of the materials is catalyst: reactant: solvent = 1:10:490. In this embodiment, the catalyst 10Ni / 40Nb@Si obtained in Example 5 is selected, the mass is 0.05 g, the reactant is guaiacol, and the solvent is n-dodecane. The pre-reaction treatment and reaction conditions are the same as in Example 6, and the conversion rate and selectivity data of the relevant species are calculated and shown in Table 2.
[0082] Example 12
[0083] Add materials into a 100 mL high pressure mechanical stirring kettle, the mass ratio of the materials is catalyst: reactant: solvent = 1:10:490. In this embodiment, the catalyst 10Ni / Nb obtained in Comparative Example 2 is selected. 2 O 5 , with a mass of 0.05 g, the reactant is guaiacol, and the solvent is n-dodecane. The pre-reaction treatment and reaction conditions are the same as those in Example 6, and the conversion rate and selectivity data of the relevant species are calculated and shown in Table 2.
[0084] From the results of different ratios, it can be seen that pure Ni / SiO 2 The catalyst has too low selectivity for cycloalkanes, and the products are mainly oxygen-containing products, indicating that the catalyst's deoxygenation ability is insufficient. After the introduction of Nb, the yield of cycloalkanes is improved. The catalytic effect shows a trend of increasing first and then decreasing with the increase of Nb content. When the Nb content is 20wt%, the corresponding catalytic activity is the highest, which can make the guaiacol conversion rate reach 100% and the selectivity of cyclohexane reach 94.37%. It shows that the appropriate amount of Nb content is conducive to the improvement of the selectivity of deoxygenated products.
[0085] Table 2 Reaction results of Examples 6-12
[0086]
[0087] In order to compare the effects of different reaction temperatures on the hydrodeoxygenation reaction of guaiacol, the catalyst 10Ni / 20Nb@Si was selected as a further research object, and the following experiments of Examples 13-19 were carried out.
[0088] Embodiment 13
[0089] Feed materials into a 100mL high-pressure mechanical stirring kettle, and the mass ratio of the materials is catalyst: reactant: solvent = 1:10:490. In this embodiment, the mass of the catalyst 10Ni / 20Nb@Si obtained in Example 3 is 0.05g, the reactant is guaiacol, and the solvent is n-dodecane. Assemble the reactor and check the airtightness of the device, then fill argon from the reaction inlet, and replace the gas in the kettle several times until the air content is negligible. Turn on the condensing water, turn on the mechanical stirring to a certain speed, set the heating program and start heating. Use 5MPa hydrogen as the hydrogen source, react at a temperature of 200℃ for 2h, and calculate the conversion rate and selectivity data of the relevant species, see Table 3.
[0090] Embodiment 14
[0091] The materials were added to a 100 mL high pressure mechanical stirring kettle, and the amounts of the catalyst and the materials used were the same as those in Example 13. 5 MPa hydrogen was used as the hydrogen source, and the reaction was carried out at a temperature of 210° C. for 2 h. The conversion rate and selectivity data of the relevant species were calculated and shown in Table 3.
[0092] Embodiment 15
[0093] The materials were added to a 100 mL high pressure mechanical stirring kettle, and the amounts of the catalyst and the materials used were the same as those in Example 13. 5 MPa hydrogen was used as the hydrogen source, and the reaction was carried out at a temperature of 220° C. for 2 h. The conversion rate and selectivity data of the relevant species were calculated and shown in Table 3.
[0094] Example 16
[0095] The materials were added to a 100 mL high pressure mechanical stirring kettle, and the amounts of the catalyst and the materials used were the same as those in Example 13. 5 MPa hydrogen was used as the hydrogen source, and the reaction was carried out at a temperature of 230° C. for 2 h. The conversion rate and selectivity data of the relevant species were calculated and shown in Table 3.
[0096] Embodiment 17
[0097] The materials were added to a 100 mL high pressure mechanical stirring kettle, and the amounts of the catalyst and the materials used were the same as those in Example 13. 5 MPa hydrogen was used as the hydrogen source, and the reaction was carried out at a temperature of 240° C. for 2 h. The conversion rate and selectivity data of the relevant species were calculated and shown in Table 3.
[0098] Embodiment 18
[0099] The materials were added to a 100 mL high pressure mechanical stirring kettle, and the amounts of the catalyst and the materials used were the same as those in Example 13. 5 MPa hydrogen was used as the hydrogen source, and the reaction was carried out at a temperature of 250° C. for 2 h. The conversion rate and selectivity data of the relevant species were calculated and shown in Table 3.
[0100] Embodiment 19
[0101] The materials were added to a 100 mL high pressure mechanical stirring kettle, and the amounts of the catalyst and the materials used were the same as those in Example 13. 5 MPa hydrogen was used as the hydrogen source, and the reaction was carried out at a temperature of 260° C. for 2 h. The conversion rate and selectivity data of the relevant species were calculated and shown in Table 3.
[0102] Table 3 Reaction results of catalyst HDO at different temperatures
[0103]
[0104] From the temperature point of view, at a lower reaction temperature, the selectivity of cycloalkanes is not high enough, and cycloalcohols and cycloethers account for a large proportion, indicating that low temperature conditions are not enough to effectively remove hydroxyl and methoxy groups. As the reaction temperature increases, the rate of removal of hydroxyl and methoxy groups gradually increases, resulting in a gradual increase in the amount of cyclohexane generated. At 250 ° C, the yield of cycloalkane products reached 100%. The sudden increase in selectivity may be because the temperature has exceeded the energy required for the breakage of the Calkyl-OH bond, causing the alcohol product to quickly remove hydroxyl groups to generate cycloalkanes. After that, the reaction temperature was raised again, and there was no obvious change in the distribution of each product.
[0105] To further compare the effects of different reaction pressures on the hydrodeoxygenation reaction of guaiacol, the following experiments of Examples 20-24 were conducted.
[0106] Embodiment 20
[0107] Feed materials into a 100mL high-pressure mechanical stirring kettle, and the mass ratio of the materials is catalyst: reactant: solvent = 1:10:490. In this embodiment, the mass of the catalyst 10Ni / 20Nb@Si obtained in Example 3 is 0.05g, the reactant is guaiacol, and the solvent is n-dodecane. Assemble the reactor and check the airtightness of the device, then fill argon from the reaction inlet, and replace the gas in the kettle several times until the air content is negligible. Turn on the condensing water, turn on the mechanical stirring to a certain speed, set the heating program and start heating. Use 2MPa hydrogen as the hydrogen source, react at a temperature of 250℃ for 2h, and calculate the conversion rate and selectivity data of related species, see Table 4.
[0108] Embodiment 21
[0109] The materials were added to a 100 mL high pressure mechanical stirring kettle. The catalyst and reaction materials were the same as those in Example 20. 3 MPa hydrogen was used as the hydrogen source and the reaction was carried out at 250° C. for 2 h. The conversion and selectivity data of the relevant species were calculated and shown in Table 4.
[0110] Embodiment 22
[0111] The materials were added to a 100 mL high pressure mechanical stirring kettle, and the amounts of the catalyst and the materials used were the same as those in Example 20. 4 MPa hydrogen was used as the hydrogen source, and the reaction was carried out at a temperature of 250° C. for 2 h. The conversion rate and selectivity data of the relevant species were calculated and shown in Table 4.
[0112] Embodiment 23
[0113] The materials were added to a 100 mL high pressure mechanical stirring kettle, and the amounts of the catalyst and the materials used were the same as those in Example 20. 5 MPa hydrogen was used as the hydrogen source, and the reaction was carried out at a temperature of 250° C. for 2 h. The conversion rate and selectivity data of the relevant species were calculated and shown in Table 4.
[0114] Embodiment 24
[0115] The materials were added to a 100 mL high pressure mechanical stirring kettle, and the amounts of the catalyst and the materials used were the same as those in Example 20. 6 MPa hydrogen was used as the hydrogen source, and the reaction was carried out at a temperature of 250° C. for 2 h. The conversion rate and selectivity data of the relevant species were calculated and shown in Table 4.
[0116] Table 4 Reaction results of catalyst HDO under different pressures
[0117]
[0118] Reaction H 2The influence of pressure on product distribution is mainly reflected in the change in the content of unsaturated products. Under relatively low pressure conditions, there is a certain amount of benzene and 1,2-dimethoxybenzene, indicating that the hydrogen source is insufficient and it is difficult for the benzene ring to be hydrogenated and saturated, so the hydrogen partial pressure should be increased. As the reaction pressure continues to increase, the selectivity of cycloalkanes reaches a peak at 5MPa, but decreases slightly at 6MPa. This is mainly because under high hydrogen pressure conditions, a part of the cycloalkanes undergo a ring contraction reaction due to C-C bond hydrogenolysis to generate methylcyclopentane.
[0119] In order to further compare the effects of different reaction times on the hydrodeoxygenation reaction of guaiacol, the following experiments of Examples 25-29 were conducted.
[0120] Embodiment 25
[0121] Feed materials into a 100mL high-pressure mechanical stirring kettle, and the mass ratio of the materials is catalyst: reactant: solvent = 1:10:490. In this embodiment, the mass of the catalyst 10Ni / 20Nb@Si obtained in Example 3 is 0.05g, the reactant is guaiacol, and the solvent is n-dodecane. Assemble the reactor and check the airtightness of the device, then fill argon from the reaction inlet, and replace the gas in the kettle several times until the air content is negligible. Turn on the condensing water, turn on the mechanical stirring to a certain speed, set the heating program and start heating. Use 5MPa hydrogen as the hydrogen source, react at a temperature of 250℃ for 0.5h, and calculate the conversion rate and selectivity data of related species, see Table 5.
[0122] Embodiment 26
[0123] The materials were added to a 100 mL high pressure mechanical stirring kettle, and the amounts of the catalyst and the materials used were the same as those in Example 25. 5 MPa hydrogen was used as the hydrogen source, and the reaction was carried out at a temperature of 250° C. for 1 h. The conversion rate and selectivity data of the relevant species were calculated and shown in Table 5.
[0124] Embodiment 27
[0125] The materials were added to a 100 mL high pressure mechanical stirring kettle. The catalyst and reaction materials were the same as those in Example 25. 5 MPa hydrogen was used as the hydrogen source and the reaction was carried out at 250° C. for 2 h. The conversion and selectivity data of the relevant species were calculated and shown in Table 5.
[0126] Embodiment 28
[0127] The materials were added to a 100 mL high pressure mechanical stirring kettle. The catalyst and reaction materials were the same as those in Example 25. 5 MPa hydrogen was used as the hydrogen source and the reaction was carried out at 250° C. for 4 h. The conversion and selectivity data of the relevant species were calculated and shown in Table 5.
[0128] Embodiment 29
[0129] The materials were added to a 100 mL high pressure mechanical stirring kettle. The catalyst and reaction materials were the same as those in Example 25. 5 MPa hydrogen was used as the hydrogen source and the reaction was carried out at 250° C. for 6 h. The conversion and selectivity data of the relevant species were calculated and shown in Table 5.
[0130] Table 5 Reaction results of catalyst HDO at different reaction times
[0131]
[0132] The change pattern of the reaction over time (0.5-6h) shows that guaiacol has been completely converted after 1h of reaction, indicating that the catalyst 10Ni / 20Nb@Si has a high catalytic efficiency and can quickly achieve hydrogenation saturation of aromatic rings and effective removal of some oxygen-containing functional groups. After that, when the time was extended to 2h, the yield of the target product has stabilized. When the time was further extended, it was found that the cycloalkane products began to gradually decrease, which was also attributed to the ring contraction reaction to generate some branched cyclopentane and cyclobutane. Overall, the optimal reaction conditions are 250℃, 5MPa, and 2h.
[0133] In order to explore the universality of the catalyst 10Ni / 20Nb@Si, it was applied to HDO experiments of other representative lignin-derived monomers and dimers. In order to study the effects of different substituents on the aromatic ring on HDO, phenol, m-cresol, p-cresol, and 2-methoxy-4-propylphenol were selected as representative model compounds. To further increase the unsaturation of the reactants, eugenol was used as a reactant. In order to study the effects of more oxygen-containing functional groups in the reactants, 2,6-dimethoxyphenol and 4-phenoxyphenol were used as reactants. Specific examples are as follows.
[0134] Embodiment 30
[0135] The catalyst 10Ni / 20Nb@Si obtained in Example 3 was used for the hydrodeoxygenation reaction of phenol. 24.5 g of n-dodecane, 4 mmol (mass 0.3760 g) of reactants and 0.05 g of catalyst were put into a reactor. The pre-reaction treatment conditions were the same as those in Example 25, the temperature was raised to 250°C, the hydrogen pressure in the reactor was maintained at 5 MPa, the reaction time was 2 h, and the conversion rate and selectivity data of the relevant species were calculated and shown in Table 6.
[0136] Embodiment 31
[0137] The obtained catalyst 10Ni / 20Nb@Si was used for the hydrodeoxygenation reaction of m-methylphenol. 24.5g of n-dodecane, 4mmol (mass 0.4326g) of reactant and 0.05g of catalyst were put into the reactor. The pre-reaction treatment conditions were the same as those in Example 25, the temperature was raised to 250°C, the hydrogen pressure in the reactor was maintained at 5MPa, the reaction time was 2h, and the conversion rate and selectivity data of the relevant species were calculated and shown in Table 6.
[0138] Embodiment 32
[0139] The obtained catalyst 10Ni / 20Nb@Si was used for the hydrodeoxygenation reaction of p-methylphenol. 24.5g of n-dodecane, 4mmol (mass 0.4326g) of reactant and 0.05g of catalyst were put into the reactor. The pre-reaction treatment conditions were the same as those in Example 25, the temperature was raised to 250°C, the hydrogen pressure in the reactor was maintained at 5MPa, the reaction time was 2h, and the conversion rate and selectivity data of the relevant species were calculated and shown in Table 6.
[0140] Embodiment 33
[0141] The obtained catalyst 10Ni / 20Nb@Si was used for the hydrodeoxygenation reaction of guaiacol. 24.5g of n-dodecane, 4mmol (mass 0.4966g) of reactant and 0.05g of catalyst were put into the reactor. The pre-reaction treatment conditions were the same as those in Example 25, the temperature was raised to 250°C, the hydrogen pressure in the reactor was maintained at 5MPa, the reaction time was 2h, and the conversion rate and selectivity data of the relevant species were calculated and shown in Table 6.
[0142] Embodiment 34
[0143] The obtained catalyst 10Ni / 20Nb@Si was used for the hydrodeoxygenation reaction of 2-methoxy-4-propylphenol. 24.5g of n-dodecane, 4mmol (mass 0.6649g) of reactant and 0.05g of catalyst were put into the reactor. The pre-reaction treatment conditions were the same as those in Example 25, the temperature was raised to 250°C, the hydrogen pressure in the reactor was maintained at 5MPa, the reaction time was 10h, and the conversion rate and selectivity data of the relevant species were calculated and shown in Table 6.
[0144] Embodiment 35
[0145] The obtained catalyst 10Ni / 20Nb@Si was used for the hydrodeoxygenation reaction of eugenol. 24.5g of n-dodecane, 4mmol (mass 0.6568g) of reactant and 0.05g of catalyst were put into the reactor. The pre-reaction treatment conditions were the same as those in Example 25, the temperature was raised to 250°C, the hydrogen pressure in the reactor was maintained at 5MPa, the reaction time was 10h, and the conversion rate and selectivity data of the relevant species were calculated and shown in Table 6.
[0146] Embodiment 36
[0147] The obtained catalyst 10Ni / 20Nb@Si was used for the hydrodeoxygenation reaction of 2,6-dimethoxyphenol. 24.5g of n-dodecane, 4mmol of phenol (mass 0.6167g), and 0.05g of catalyst were put into the reactor. The pre-reaction treatment conditions were the same as those in Example 25, the temperature was raised to 250°C, the hydrogen pressure in the reactor was maintained at 5MPa, the reaction time was 10h, and the conversion rate and selectivity data of the relevant species were calculated and shown in Table 6.
[0148] Embodiment 37
[0149] The obtained catalyst 10Ni / 20Nb@Si was used for the hydrodeoxygenation reaction of 4-phenoxyphenol. 24.5g of n-dodecane, 4mmol (mass 0.7448g) of reactant and 0.05g of catalyst were put into the reactor. The pre-reaction treatment conditions were the same as those in Example 25, the temperature was raised to 250°C, the hydrogen pressure in the reactor was maintained at 5MPa, the reaction time was 10h, and the conversion rate and selectivity data of the relevant species were calculated and shown in Table 6.
[0150] Table 6 Reaction results of Examples 30-37
[0151]
[0152]
[0153] The present invention is described in detail above with specific embodiments. Obviously, the described examples are only a part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0154] Matters not covered by the present invention are known technologies.
Claims
1. A method for preparing a hydrodeoxygenation bifunctional NiNb-based catalyst, The method is characterized in that it comprises the following steps: (1) adding a silicon source to deionized water, stirring magnetically for 5-30 minutes, then adding a complexing agent, and continuing to stir magnetically for 5-30 minutes to obtain a solution A; The mass ratio of the added components is silicon source: complexing agent: deionized water = 1:0.1-0.5:4-12; (2) adding the niobium source to the solution A obtained in step (1) under stirring, and continuing magnetic stirring for 2-8 hours to obtain a homogeneous hydrogel prepolymer solution B; Wherein, the mass ratio is niobium source:silicon source=1:1-21; (3) drying the hydrogel prepolymer solution B obtained in step (2) in stages, wherein the first stage is drying at a constant temperature of 40-60° C. for 4-6 hours, taking out and grinding; and then drying at a constant temperature of 40-60° C. for another 4-6 hours to obtain a dry solid; (4) calcining the dried solid obtained in step (3) at 400-600° C. for 3-5 h at a heating rate of 1-5° C. / min to obtain a niobium-doped silica composite oxide support; (5) measuring the saturated water absorption of the composite oxide support obtained in step (4), and then dripping the nickel source solution onto the support by an equal amount impregnation method; (6) drying the sample obtained in step (5) at 30-40° C. for 10-12 h; (7) calcining the dried sample in step (6) at 400-600° C. for 3-5 h; (8) The sample calcined in step (7) is reduced in a tubular furnace in a flowing hydrogen atmosphere at 400-600° C. for 3-5 h to obtain an xNi / yNb@Si catalyst, i.e., a hydrogenation and deoxygenation bifunctional NiNb-based catalyst.
2. The method for preparing the hydrodeoxygenation bifunctional NiNb-based catalyst according to claim 1, characterized in that The silicon source in step (1) is one or more of ethyl orthosilicate, methyl orthosilicate, butyl orthosilicate, isopropyl orthosilicate and alkyl alkoxy silane.
3. The method for preparing the hydrodeoxygenation bifunctional NiNb-based catalyst according to claim 1, characterized in that The complexing agent in step (1) includes one or more of citric acid, tartaric acid, ethylenediaminetetraacetic acid, malic acid, glycolic acid, and succinic acid.
4. The method for preparing the hydrodeoxygenation bifunctional NiNb-based catalyst according to claim 1, characterized in that The niobium source in step (2) includes one or more of niobium oxalate, niobium pentachloride, niobium ethoxide, niobium acetate, ammonium niobate oxalate hydrate or niobium hydroxide.
5. The method for preparing the hydrodeoxygenation bifunctional NiNb-based catalyst according to claim 1, characterized in that The nickel source in step (5) includes one or more of nickel nitrate, nickel chloride, nickel carbonate and nickel oxalate; the concentration of the nickel source solution is 1-4 mol / L.
6. Use of the hydrodeoxygenation bifunctional NiNb-based catalyst prepared by the method of claim 1, characterized in that it is used as a catalyst in the process of preparing cycloalkane fuel by hydrodeoxygenation reaction of lignin derivatives.
7. The use according to claim 6, characterized in that it comprises the following steps: A lignin derivative, n-dodecane and a hydrodeoxygenation bifunctional NiNb-based catalyst are added to a reaction kettle, which is sealed and replaced with 0.5-2 MPa argon gas in the kettle, and then reacted for 0.5-10 hours at a hydrogen pressure of 3-7 MPa, 200-260° C. and stirring to obtain cycloalkanes; in, The mass ratio of feed is catalyst: reactant: solvent = 1: 5-100: 490-2400; The lignin derivative is one or more of lignin-derived phenolic substances and lignin-derived dimer substances.
8. The use according to claim 7, characterized in that The lignin derivative is one or more of phenol, m-cresol, p-cresol, guaiacol, 2-methoxy-4-propylphenol, eugenol, 2,6-dimethoxyphenol and lignin-derived dimer substances containing β-O-4, α-O-4 and 4-O-5 bonds.
Citation Information
Patent Citations
Method of preparing hydrocarbon fuel through hydrotreating lignin depolymerization lightweight phenolic product
CN106753549A
Hydrodeoxygenation catalyst and preparation method and application thereof
CN113441139A
Preparation method and application of Pt / AlSiO-Nb hydrodeoxygenation coupling isomerization catalyst
CN116943649A
Cited By
Process for preparing biological aviation kerosene from waste oil
CN121294022A