High-performance low-anisotropy flange production process
By employing specific forging and heat treatment processes, the anisotropy problem of flange parts materials has been solved, enabling the production of high-performance, low-anisotropy flanges and improving the overall mechanical properties of the materials.
Patent Information
- Application Number
- CN202411402278.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-09
- Publication Date
- 2024-11-22
AI Technical Summary
In the manufacture of flange parts, existing technologies have large differences in the three-dimensional properties of materials, making it difficult to achieve high performance with low anisotropy.
By employing specific forging and heat treatment processes, including forging heating, multiple axial and radial upsetting and drawing, solution treatment, and aging treatment, the grains are refined and a uniform strengthening phase network is formed by creating crisscrossing deformation bands and dislocation cells within the material.
It significantly improves the tensile strength, elongation and other mechanical properties of flange parts, reduces the anisotropy of the material, and improves the overall performance of the material.
Smart Images

Figure CN118989207A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum alloy forging, and in particular to a high-performance, low-anisotropy flange production process. Background Art
[0002] Aluminum (Al) alloy is one of the lightest structural metals. It has great potential to improve energy efficiency in the fields of aerospace, electronics, automobiles and defense due to its low density, high strength, easy recycling and outstanding corrosion resistance. 2A14 aluminum alloy belongs to the A1-Cu-Mg-Si series forging alloy, also known as high-strength forged aluminum. It is an alloy developed by adding Si to the A1-Cu-Mg hard aluminum alloy to improve its processing performance. 2A14 aluminum alloy is suitable for manufacturing complex-shaped free forgings and precision die forgings due to its high strength, good thermoplasticity, good forging, high operating temperature and good welding performance.
[0003] Currently, a certain type of flange parts needs to be manufactured. The current process is multiple axial upsetting and drawing, followed by punching and ring rolling. The three-dimensional performance of the material varies greatly.
[0004] It should be noted that the information disclosed in the above background technology section is only used to enhance the understanding of the background of the present disclosure, and therefore may include information that does not constitute the prior art known to ordinary technicians in the field. Summary of the invention
[0005] Aiming at the deficiencies of the prior art, the present invention is disclosed.
[0006] The technical solution adopted by the present invention is as follows:
[0007] A high-performance, low-anisotropy flange production process, characterized in that it includes the following steps: step S1, raw material preparation; step S2, material cutting; step S3, forging, including the following steps: (1) forging heating: heating the raw material to 460±10°C for heat preservation; (2) forging: axial "Z" upsetting, axial "Z" stretching, axial "Z" upsetting, radial "X" stretching, radial "X" upsetting, radial "X" stretching, radial "X" upsetting, radial "Y" drawing, radial "Y" upsetting, radial "Y" drawing, radial "Y" upsetting, axial "Z" drawing, axial "Z" upsetting, axial "Z" drawing and axial "Z" rolling, the final forging temperature is ≥360℃; (3) cooling after forging; step S4, heat treatment, including the following steps: (1) solution treatment: heating the forging to 490-510℃ and keeping it warm, and then cooling the forging; (2) aging: heating the forging to 155-165℃ and keeping it warm, and then cooling the forging.
[0008] Furthermore, in step S1, the raw materials include the element contents calculated by mass fraction: Si, 0.6-1.2%; Fe, 0.7%; Cu, 3.9-4.8%; Mn, 0.4-1; Mg, 0.4-0.8; Ni, 0.1%; Zn, 0.3; Ti, 0.15, other impurities totaling 0.15%, and the balance being Al.
[0009] Furthermore, in the pre-forging heating of step S2, the holding time of the hot material is calculated based on the effective thickness of the billet, and the calculation standard is 0.8 min / mm; the holding time of the cold material is calculated based on the effective thickness of the billet, and the calculation standard is 1.8 min / mm.
[0010] Furthermore, in the forging of step S2, the initial forging temperature ranges from 420 to 460°C.
[0011] Furthermore, in the forging of step S2, the hammer head presses down at a speed of 10 to 20 mm / s.
[0012] Furthermore, in the forging of step S2, the lower limit of the tooling temperature is 200°C, and the upper limit of the tooling temperature is 350°C.
[0013] Furthermore, in the solid solution of step S2, the heat preservation time is 6 to 11 hours.
[0014] Furthermore, in the solid solution of step S2, the cooling medium is water, the upper limit of the cooling medium temperature is room temperature, and the cooling immersion time ranges from 30 minutes to 45 minutes.
[0015] Furthermore, in the aging process of step S2, the heat preservation time ranges from 4 to 6 hours.
[0016] Furthermore, in the aging process of step S2, the interval between solution treatment and aging is less than 3 hours.
[0017] The beneficial effects of the present invention are as follows:
[0018] 1. During the deformation process of forgings, the repeated upsetting and elongation of the block material can be achieved by continuously reversing along the three axes of x, y and z, and criss-crossing deformation bands are formed inside the material. Dislocations are seriously accumulated at the intersection of the deformation bands and form dislocation cells through interaction. When the deformation continues, the dislocation cells gradually develop into subgrains with independent slip systems. Through the absorption of dislocations by subgrain boundaries, subgrains with small-angle grain boundaries are transformed into new grains with large-angle grain boundaries, thereby achieving grain refinement, effectively improving the mechanical properties of forgings such as tensile strength and elongation, and reducing the difference in their three-dimensional properties.
[0019] 2. Heating to the appropriate temperature window before forging allows some elements in the alloy to begin to dissolve into the matrix, mainly to obtain good thermoplasticity and lower deformation resistance, so that plastic deformation is easier during the forging process; and to ensure the final forging temperature. Maintaining a higher final forging temperature can ensure that the alloy still maintains good plasticity and lower deformation resistance during the deformation process, which helps to reduce the internal stress generated by the alloy during the forging process and avoid deformation or cracking of the forging due to the release of internal stress during the cooling process.
[0020] 3. During the solid solution process, the atomic diffusion rate is accelerated, the dissolution of the second phase is promoted, and the excess phase is fully dissolved into the solid solution and then quickly cooled. The structure is mainly composed of α-Al matrix and a small amount of dispersed strengthening phase, forming a finer and more evenly distributed strengthening phase network, thereby significantly improving the mechanical properties of the alloy.
[0021] 4. During the aging process, the supersaturated solid solution in the alloy will gradually decompose and precipitate strengthening phases such as S' phase and Ω phase. The formation of these strengthening phases will hinder the movement of dislocations. The organization is mainly composed of α-Al matrix and dispersed strengthening phases. With the increase of aging temperature and the extension of time, the number and size of strengthening phases will gradually increase. These strengthening phases are usually distributed in the matrix in the form of fine needles, flakes or particles, forming a strengthening phase network, which can significantly improve the strength and hardness of the alloy while maintaining good plasticity and toughness. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a schematic diagram of the steps of the production process of the high-performance, low-anisotropy 2A14 flange of the present invention. DETAILED DESCRIPTION
[0023] The specific implementation of the present invention will be described below in conjunction with the accompanying drawings.
[0024] Embodiment 1:
[0025] A high performance low anisotropy flange production process, such as Figure 1 As shown, the following steps are included:
[0026] Step S1, raw material preparation, the raw materials include the element content calculated by mass fraction: Si, 0.6-1.2%; Fe, 0.7%; Cu, 3.9-4.8%; Mn, 0.4-1; Mg, 0.4-0.8; Ni, 0.1%; Zn, 0.3; Ti, 0.15, other impurities totaling 0.15%, and the balance being Al.
[0027] Step S2, cutting, cutting size: Φ500mm×746(+5 / 0)mm, cutting weight: 410(+5 / -5)kg.
[0028] Step S3, forging, includes the following steps:
[0029] (1) Forging heating: The raw material is heated to 460±10℃ and kept warm; Heating and insulation coefficient: When heating, the insulation time of cold material is calculated as 1.6min / mm, and the insulation time of hot material (when the return temperature is ≥300℃) is calculated as 0.8min / mm. The effective thickness of the billet is used as the calculation basis, which is generally the smaller of the thickness and height.
[0030] (2) Forging:
[0031] Initial forging temperature of billet: 440~460℃. Preheat the tooling in advance, the temperature range is 300~420℃.
[0032] Axial "Z" upsetting: upsetting to height = 550 ± 10mm; after upsetting, use a marker to mark "Z" on the end face to distinguish between axial and radial directions.
[0033] Axial "Z" stretching: Square it according to the original axial direction and stretch it to 400mm*910mm. After squaring, use a marker to mark "X" and "Y" in the original radial direction respectively.
[0034] Axial “Z” upsetting: Upsetting to height = 500 ± 10 mm.
[0035] Radial “X” stretching: stretch in “X” direction to 400mm*910mm.
[0036] Radial “X” upsetting: Upsetting to height = 500 ± 10 mm.
[0037] Radial “X” stretching: stretch in “X” direction to 400mm*910mm.
[0038] Radial “X” upsetting: Upsetting to height = 500 ± 10 mm.
[0039] Radial “Y” stretching: stretch in “Y” direction to 400mm*910mm.
[0040] Radial “Y” upsetting: upsetting to height = 500 ± 10 mm.
[0041] Radial “Y” stretching: stretch in “Y” direction to 400mm*910mm.
[0042] Radial “Y” upsetting: upsetting to height = 500 ± 10 mm.
[0043] Axial "Z" stretching: stretch in "Z" direction to 400mm*910mm.
[0044] Axial “Z” upsetting: Upsetting to height = 500 ± 10 mm.
[0045] Axial "Z" stretching: stretch in "Z" direction to 320mm*1430mm.
[0046] The axial "Z" is rolled to Φ350±5mm×1500±30mm.
[0047] Ensure that the final forging temperature of the forging is ≥370mm. If the temperature is lower than the final forging temperature, the direction must be marked and then returned to the furnace for heating, and kept warm for 1 to 3 hours before being taken out of the furnace for forging.
[0048] After forging is completed, the forging is air-cooled and transferred to the next step. The forging transfer time is ≤90s.
[0049] Step S4: heat treatment:
[0050] (1) Solution treatment: heat the forging to 495℃ and keep it for 6h. Then cool the forging. Cooling medium: water. Upper limit of cooling medium temperature: room temperature. Upper limit of immersion time: 45min. Lower limit of immersion time: 30min. Heat treatment transfer time ≤15s.
[0051] (2) Aging: Heat the forgings to 155℃ and keep them warm for 5 hours, then take them out of the furnace and air cool them.
[0052] The time interval between aging treatment and solution treatment is less than 3h.
[0053] Comprehensive product performance testing:
[0054] Sampling: As a product is drawn, two sampling points are taken in the longitudinal, transverse and height directions respectively.
[0055] Test equipment: microcomputer controlled electronic universal testing machine and extensometer.
[0056] Test conditions: GB / T228A223.
[0057] Test temperature: 22.5.
[0058] The test results are shown in Table 1:
[0059]
[0060] Table 1
[0061] Embodiment 2:
[0062] A high performance low anisotropy flange production process, such as Figure 1 As shown, the following steps are included:
[0063] Step S1, raw material preparation, the raw materials include the element content calculated by mass fraction: Si, 0.6-1.2%; Fe, 0.7%; Cu, 3.9-4.8%; Mn, 0.4-1; Mg, 0.4-0.8; Ni, 0.1%; Zn, 0.3; Ti, 0.15, other impurities totaling 0.15%, and the balance being Al.
[0064] Step S2, cutting, cutting size: Φ500mm×346(+5 / 0)mm, cutting weight: 190(+5 / -5)kg.
[0065] Step S3, forging, includes the following steps:
[0066] (1) Forging heating: The raw material is heated to 460±10℃ and kept warm; Heating and insulation coefficient: When heating, the insulation time of cold material is calculated as 1.6min / mm, and the insulation time of hot material (when the return temperature is ≥300℃) is calculated as 0.8min / mm. The effective thickness of the billet is used as the calculation basis, which is generally the smaller of the thickness and height.
[0067] (2) Forging:
[0068] Initial forging temperature of billet: 440~460℃. Preheat the tooling in advance, the temperature range is 300~420℃.
[0069] Axial "Z" upsetting: upsetting to height = 330 ± 10mm; after upsetting, mark "Z" on the end face with a marker to distinguish between axial and radial directions.
[0070] Axial "Z" stretching: Square it according to the original axial direction and stretch it to ~320mm*660mm. After squaring, use a marker to mark "X" and "Y" in the original radial direction respectively.
[0071] Axial “Z” upsetting: Upsetting to height = 400 ± 10 mm.
[0072] Radial “X” stretching: stretch in “X” direction to 320mm*660mm.
[0073] Radial “X” upsetting: Upsetting to height = 400 ± 10 mm.
[0074] Radial “X” stretching: stretch in “X” direction to 320mm*660mm.
[0075] Radial “X” upsetting: Upsetting to height = 400 ± 10 mm.
[0076] Radial “Y” stretching: stretch in “Y” direction to 320mm*660mm.
[0077] Radial “Y” upsetting: upsetting to height = 400 ± 10 mm.
[0078] Radial “Y” stretching: stretch in “Y” direction to 320mm*660mm.
[0079] Radial “Y” upsetting: upsetting to height = 400 ± 10 mm.
[0080] Axial "Z" stretching: stretch in "Z" direction to 320mm*660mm.
[0081] Axial “Z” upsetting: Upsetting to height = 400 ± 10 mm.
[0082] Axial "Z" stretching: stretch in "Z" direction to 185mm*1900mm.
[0083] Axial "Z" chamfering and rounding to Φ200(+5 / 0)mm×2000±30mm.
[0084] Ensure that the final forging temperature of the forging is ≥370mm. If the temperature is lower than the final forging temperature, the direction must be marked and then returned to the furnace for heating, and kept warm for 1 to 3 hours before being taken out of the furnace for forging.
[0085] After forging is completed, the forging is air-cooled and transferred to the next step. The forging transfer time is ≤90s.
[0086] Step S4: heat treatment:
[0087] (1) Solution treatment: the forging is heated to 505℃ and kept at this temperature for 6 hours. After that, the forging is cooled. The cooling medium is water. The upper limit temperature of the cooling medium is room temperature. The upper limit of the immersion time is 45 minutes. The lower limit of the immersion time is 30 minutes. The heat treatment transfer time is ≤ 15 seconds.
[0088] (2) Aging: Heat the forgings to 165℃ and keep them warm for 5 hours, then take them out of the furnace and air cool them.
[0089] The time interval between aging treatment and solution treatment is less than 3h.
[0090] Comprehensive product performance testing:
[0091] Sampling: As a product is drawn, two sampling points are taken in the longitudinal, transverse and height directions respectively.
[0092] Test equipment: microcomputer controlled electronic universal testing machine and extensometer.
[0093] Test conditions: GB / T228A223.
[0094] Test temperature: 22.5.
[0095] The test results are shown in Table 2:
[0096]
[0097] Table 2
[0098] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0099] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A high-performance, low-anisotropy flange production process, characterized in that: The following steps are involved: Step S1, raw material preparation; Step S2, blanking; Step S3, forging, includes the following steps: (1) Forging heating: The raw material is heated to 460±10℃ and kept warm; (2) Forging: axial "Z" upsetting, axial "Z" drawing, axial "Z" upsetting, radial "X" drawing, radial "X" upsetting, radial "X" drawing, radial "X" upsetting, radial "Y" drawing, radial "Y" upsetting, radial "Y" drawing, radial "Y" upsetting, axial "Z" drawing, axial "Z" upsetting, axial "Z" drawing and axial "Z" rolling in sequence, with the final forging temperature ≥ 360℃; (3) Cooling after forging; Step S4, heat treatment, includes the following steps: (1) Solution treatment: The forging is heated to 490-510℃ and then cooled; (2) Aging: The forging is heated to 155-165°C and kept warm, then cooled.
2. A high-performance, low-anisotropy flange production process according to claim 1, characterized in that: In step S1, the raw material includes the following element contents calculated by mass fraction: Si, 0.6-1.2%; Fe, 0.7%; Cu, 3.9-4.8%; Mn, 0.4-1; Mg, 0.4~0.8; Ni, 0.1%; Zn, 0.3; Ti, 0.15, other impurities total 0.15%, and the balance is Al.
3. A high-performance, low-anisotropy flange production process according to claim 1, characterized in that: In the pre-forging heating of step S2, the holding time of the hot material is calculated based on the effective thickness of the billet, and the calculation standard is 0.8 min / mm; the holding time of the cold material is calculated based on the effective thickness of the billet, and the calculation standard is 1.8 min / mm.
4. A high-performance, low-anisotropy flange production process according to claim 1, characterized in that: In the forging of step S2, the initial forging temperature ranges from 420 to 460°C.
5. A high-performance, low-anisotropy flange production process according to claim 4, characterized in that: In the forging of step S2, the hammer head presses down at a speed of 10 to 20 mm / s.
6. A high-performance, low-anisotropy flange production process according to claim 5, characterized in that: In the forging of step S2, the lower limit of the tooling temperature is 200°C, and the upper limit of the tooling temperature is 350°C.
7. The high-performance, low-anisotropy flange production process according to claim 1, characterized in that: In the solid solution of step S2, the holding time is 6 to 11 hours.
8. The high-performance, low-anisotropy flange production process according to claim 7, characterized in that: In the solid solution of step S2, the cooling medium is water, the upper limit of the cooling medium temperature is room temperature, and the cooling immersion time ranges from 30 minutes to 45 minutes.
9. The high-performance, low-anisotropy flange production process according to claim 1, characterized in that: In the aging process of step S2, the temperature keeping time ranges from 4 to 6 hours.
10. A high performance, low anisotropy flange production process according to claim 9, characterized in that: In the aging process of step S2, the interval between solution treatment and aging is less than 3 hours.
Citation Information
Patent Citations
Manufacturing process of 6082 aluminum alloy flange
CN107779694A
Forming method for improving three-direction performance of aluminum alloy
CN112439857A
Production method of aluminum alloy forge piece
CN117399541A
Production of aluminum forged product having fine structure
JP1997249951A
Cited By
Processing technology of high-temperature-resistant hubbed flat welding flange
CN120395344A