Rare earth modified ceramsite precoated sand for 3D printing and preparation method of rare earth modified ceramsite precoated sand
By using the combination of quartz sand with rare earth modified ceramic particles and modified resin, the cost and efficiency problems of traditional sand mold manufacturing methods are solved, the performance and accuracy of 3D printed coated sand are improved, and the high-quality needs of complex castings are met.
Patent Information
- Application Number
- CN202411211508.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-22
AI Technical Summary
Traditional sand-form manufacturing methods have problems such as long processing cycle, high economic cost and cumbersome process when producing large and complex castings. 3D printing of coated sand requires more fine raw materials and complex processing processes, making it difficult to meet sintering performance, printing accuracy and surface. High quality requirements.
Quartz sand and rare earth modified ceramic particles are used as aggregates, combined with thermoplastic phenolic resin and rosin modified resin as binders, and high-performance rare earth modified ceramic particles are prepared through specific ratios and process flows, and the use of Materials such as cerium fluoride, lanthanum oxide, yttrium modified ceratops and concave and concave rock stone clay fly ash improve powder flowability and sintering density, and build a complex resin network structure to enhance the overall strength of the coated sand.
It significantly reduces the aggregate cost, improves the density and printing accuracy of the coated sand, ensures the dimensional accuracy and surface quality of the castings, and meets the high-performance needs of 3D-printed coated sand.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of coated sand production, and specifically relates to rare earth modified ceramsite coated sand for 3D printing and a preparation method thereof. Background Art
[0002] With the continuous advancement of science and technology and the transformation and upgrading of the global manufacturing industry, 3D printing technology, as an important representative of advanced manufacturing technology, is gradually showing its unique advantages and application potential in various fields. 3D printing technology can manufacture parts and products with complex structures by stacking materials layer by layer, greatly improving the flexibility of design and manufacturing. In recent years, with the advancement of materials science, the types of 3D printing materials have become increasingly rich, from the initial polymer materials to inorganic non-metallic materials such as metals and ceramics. The application of these materials has greatly expanded the application scope of 3D printing technology.
[0003] In the foundry industry, coated sand is widely used in the production of castings as an important molding material. Coated sand refers to sand with a layer of polymer resin film compositely coated on the surface of the sand, which has excellent molding performance and strength. In recent years, with the continuous development of casting technology and the improvement of casting quality requirements, coated sand technology has developed rapidly. In particular, with the increasing demand for high-performance and high-quality castings in important fields such as domestic automobiles, railway transportation, and aerospace, the market demand for coated sand has also continued to grow.
[0004] However, the traditional sand mold manufacturing method has problems such as long processing cycle, high economic cost, and complicated production process, especially when producing large and complex castings. The introduction of 3D printing technology has brought revolutionary changes to sand mold manufacturing. Compared with traditional sand mold manufacturing, 3D printing coated sand can achieve high-precision manufacturing of complex structures, ensure the dimensional accuracy and surface quality of castings, and greatly shorten the manufacturing cycle, improve production efficiency, reduce intermediate links, reduce scrap rate, and effectively reduce production costs. At the same time, 3D printing coated sand requires more sophisticated raw material selection and more complex processing technology. In order to meet sintering performance, printing accuracy and surface quality, it has high requirements in powder flow, uniform powder spreading, and dense sintering. Based on this, it is of great significance to study a high-performance coated sand that can be used for 3D printing. Summary of the invention
[0005] In view of the content of the background technology, the purpose of the present invention is to provide a rare earth modified ceramsite coated sand for 3D printing and a preparation method thereof. The present invention uses quartz sand and rare earth modified ceramsite as aggregates, and thermoplastic phenolic resin and rosin modified resin as binders to prepare a high-performance coated sand that can be used for 3D printing.
[0006] The present invention adopts the following technical solution: The present invention provides a rare earth modified ceramsite coated sand for 3D printing, which comprises the following preparation raw materials in parts by weight: 110-120 parts of quartz sand, 10-20 parts of modified ceramsite, 3-4.5 parts of thermoplastic phenolic resin, 1-2 parts of rosin modified resin, 1-1.4 parts of methenamine, Calcium stearate 1.2-1.8 parts, Coupling agent 0.2-0.3 parts.
[0007] Preferably, the modified ceramsite is a rare earth modified ceramsite obtained by modifying ceramsite with cerium fluoride, lanthanum oxide and yttrium fluoride; the preparation method of the rare earth modified ceramsite is: taking cerium fluoride, lanthanum oxide and yttrium fluoride, mixing and dispersing them in deionized water, adding ceramsite, stirring and ultrasonicating, and filtering; filtering the obtained dispersion liquid, recycling and reusing it, and drying the obtained ceramsite and transferring it to a muffle furnace for roasting to obtain the rare earth modified ceramsite.
[0008] Preferably, the ratio of cerium fluoride, lanthanum oxide and yttrium fluoride is 1:(0.2-0.5):0.4.
[0009] Preferably, the calcination temperature is 800-1000° C. and the calcination time is 2-4 h.
[0010] Preferably, the preparation method of the ceramsite is: taking attapulgite clay and fly ash and mixing them thoroughly, then transferring the obtained mixture into an extrusion granulator for granulation, and finally roasting at 650-800°C for 3-6 h to obtain ceramsite with a porous structure; wherein the mass ratio of attapulgite clay to fly ash is (2-3):20.
[0011] The present invention adopts fly ash as the main raw material supplemented with attapulgite clay to make ceramsite, which can fully utilize industrial waste and reduce the cost of raw materials. Attapulgite clay is a layered chain structure of magnesium-rich aluminum silicate clay, which has the characteristics of fine soil, viscosity and plasticity when wet, and can not only improve the particle strength, adhesion and porosity of the prepared ceramsite, but also promote the bonding of raw materials. The present invention further adopts cerium fluoride, lanthanum oxide and yttrium fluoride to modify the prepared ceramsite, and cerium fluoride, lanthanum oxide and yttrium fluoride are used as modifiers in a certain ratio. Under stirring and ultrasonic auxiliary conditions, the above modifier can fully penetrate into the inner surface layer of the ceramsite, react with the ceramsite matrix through subsequent roasting, and then improve the pore structure and surface properties of the ceramsite. The rare earth modified ceramsite prepared by the present invention can promote the interface bonding between the binder and the sand particles, thereby significantly improving the density of the coated sand, and at the same time has a positive impact on the microstructure of the prepared coated sand and refines the grains; the rare earth modified ceramsite and quartz sand are used as aggregates to meet the requirements of 3D printing powder flow and sintering density, and can effectively improve printing accuracy and surface quality.
[0012] Preferably, the rosin-modified resin consists of rosin-modified epoxy resin and rosin-modified phenolic resin, and the mass ratio of the two is 10:(3-5).
[0013] Preferably, the preparation method of the rosin-modified epoxy resin is: take equal masses of rosin and soybean oil acid and mix them evenly at 120-140° C., then add 5-6 times the total mass of epoxy resin, stir at 170-190° C. for 4-5 h, cool after the reaction, wash, filter and dry to obtain the product.
[0014] In view of the more complex sand mold manufacturing process of 3D printing coated sand, the present invention uses a combination of traditional thermoplastic phenolic resin, rosin-modified epoxy resin and rosin-modified phenolic resin as a binder. The active groups of the rosin-modified epoxy resin and the rosin-modified phenolic resin can react with each other to form a complex network structure. The constructed phenolic epoxy coated sand resin system has excellent flexibility and adhesion, thereby improving the overall strength of the coated sand.
[0015] The present invention also provides a method for preparing the rare earth modified ceramsite coated sand for 3D printing, comprising the following steps: Step 1: Weigh all the raw materials according to the formula, mix the quartz sand and modified ceramsite thoroughly, heat to 100-110℃ and transfer to the sand mixer; Step 2: Add thermoplastic phenolic resin, rosin modified resin and coupling agent into the sand mixer, heat to 125-145℃ and mix the sand for 3-4 minutes; Step 3: When the mixture from step 2 is cooled to 105-115°C, add hexamethylenetetramine to the sand mixer and mix for 1-1.5 minutes; Step 4: After the mixture in step 3 is cooled to 95-105°C, calcium stearate is added and the sand is mixed for 30 seconds. When the temperature of the mixture reaches 80-85°C, the material is discharged, crushed and sieved to obtain coated sand.
[0016] Preferably, the quartz sand needs to be processed into a nearly spherical shape before mixing, the AFS particle size of the quartz sand is 60-70, and the AFS particle size of the modified ceramsite is 75-85.
[0017] The beneficial effects of the present invention are: 1. The present invention uses fly ash, an industrial waste, as a raw material to prepare expanded clay, and a small amount of the obtained modified expanded clay is mixed with traditional quartz sand as aggregate, which significantly reduces the cost of aggregate. At the same time, the modified expanded clay can also promote the interface bonding between the binder and the sand particles, thereby significantly improving the density of the prepared coated sand.
[0018] 2. The present invention uses cerium fluoride, lanthanum oxide, and yttrium fluoride as modifiers with an optimized ratio, which effectively improves the pore structure and surface properties of ceramsite, and is beneficial to improving powder flowability and sintering density.
[0019] 3. The present invention combines traditional phenolic resin with rosin-modified epoxy resin and rosin-modified phenolic resin to form a binder, which can not only reduce the gas emission, but also construct a resin system with excellent flexibility and adhesion, further improving the overall strength of the coated sand. DETAILED DESCRIPTION
[0020] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme of the present invention will be clearly and completely described below in conjunction with the embodiments. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.
[0021] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0022] In the following experiments, the main components of attapulgite clay are: SiO2 53.36%, Al2O3 21.07%, Fe2O3 5.11%, CaO 0.52%, TiO2 0.17%, MgO 7.43%, Na2O 0.77%, and K2O 0.51%; the main components of fly ash are: SiO2 46.92%, Al2O3 29.58%, CaO 10.22%, MgO 2.91%, Fe2O3 6.74%, R2O 1.87%, and SO3 0.42%.
[0023] Example 1 A rare earth modified ceramsite coated sand for 3D printing, the preparation method comprising: 1. Take attapulgite clay powder and fly ash in a mass ratio of 1:8 and mix them thoroughly. Transfer the mixture into an extrusion granulator for granulation, and then place it in a furnace for calcination at 750℃ for 4 hours to obtain spherical ceramsite with a porous structure. Weigh cerium fluoride, lanthanum oxide, and yttrium fluoride in a mass ratio of 1:0.32:0.4 as a modifier, take 100 parts of the above ceramsite and 1 part of the modifier, disperse the modifier in deionized water, add ceramsite, stir and ultrasonicate (ultrasonic power 35 W, every 5 minutes of ultrasound interval 1 hour, 100 rpm continuous stirring for 12 hours); adjust the pore size of the filter medium, separate the ceramsite and the modifier dispersion, recycle the obtained dispersion, and after the ceramsite is dried, transfer it to a muffle furnace and roast it at 900℃ for 3 hours to obtain modified ceramsite (AFS particle size 75-85).
[0024] 2. Take equal masses of yellow rosin (first grade) and soybean oil acid (saponification value 205 mg / g), heat to 130℃ and mix evenly, then add E44 bisphenol A epoxy resin which is 5 times of the total mass of the two, stir at 180℃ for 4 h, cool after the reaction, wash, filter and dry to obtain rosin-modified epoxy resin; take the obtained rosin-modified epoxy resin and rosin-modified phenolic resin 2112 (purchased from Shangrao Sinan) in a mass ratio of 10:4 to form rosin-modified resin.
[0025] 3. Weigh 115 parts of quartz sand (SiO2 content 96%, AFS particle size 60-70), 15 parts of the above modified ceramsite, 3.5 parts of thermoplastic phenolic resin PF-1904, 1.5 parts of the above rosin modified resin, 1.2 parts of urotropine (40% by mass hexamethylenetetramine aqueous solution), 1.6 parts of calcium stearate, and 0.3 parts of KH550 by weight. Mix the quartz sand and modified ceramsite thoroughly, heat to 105°C and transfer to a sand mixer; continue to add thermoplastic phenolic resin, rosin modified resin and KH550, heat to 135°C and mix for 4 minutes; when the mixture is cooled to 110°C, add urotropine to the sand mixer and mix for 1.2 minutes; when the mixture is cooled to 100°C, add calcium stearate and continue mixing for 30 seconds, and when the mixture temperature reaches 85°C, discharge the material, crush and screen to obtain coated sand.
[0026] Example 2 A rare earth modified ceramsite coated sand for 3D printing, the preparation method comprising: 1. Take attapulgite clay powder and fly ash in a mass ratio of 1:10 and mix them thoroughly. Transfer the mixture into an extrusion granulator for granulation, and then place it in a furnace for calcination at 750℃ for 5 h to obtain spherical ceramsite with a porous structure. Weigh cerium fluoride, lanthanum oxide, and yttrium fluoride in a mass ratio of 1:0.5:0.4 as a modifier, take 100 parts of the above ceramsite and 1 part of the modifier, disperse the modifier in deionized water, add ceramsite, stir and ultrasonicate (ultrasonic power 35 W, every 5 min of ultrasonication, 1 h interval, 100 rpm continuous stirring for 12 h); adjust the pore size of the filter medium, separate the ceramsite and the modifier dispersion, recycle the obtained dispersion, and after the ceramsite is dried, transfer it to a muffle furnace and roast it at 800℃ for 4 h to obtain modified ceramsite (AFS particle size 75-85).
[0027] 2. Take equal masses of yellow rosin (first grade) and soybean oil acid (saponification value 205 mg / g), heat to 130℃ and mix evenly, then add E44 bisphenol A epoxy resin which is 6 times of the total mass of the two, stir at 170℃ for 5 h, cool after the reaction, wash, filter and dry to obtain rosin-modified epoxy resin; take the obtained rosin-modified epoxy resin and rosin-modified phenolic resin 2112 (purchased from Shangrao Sinan) in a mass ratio of 2:1 to form rosin-modified resin.
[0028] 3. Weigh 110 parts of quartz sand (SiO2 content 96%, AFS particle size 60-70), 20 parts of the above modified ceramsite, 4.5 parts of thermoplastic phenolic resin PF-1904, 1 part of the above rosin modified resin, 1.2 parts of urotropine (40% by mass hexamethylenetetramine aqueous solution), 1.6 parts of calcium stearate, and 0.3 parts of KH550 by weight. Mix the quartz sand and modified ceramsite thoroughly, heat to 105°C and transfer to a sand mixer; continue to add thermoplastic phenolic resin, rosin modified resin and KH550, heat to 140°C and mix for 3 minutes; when the mixture is cooled to 110°C, add urotropine to the sand mixer and mix for 1.2 minutes; when the mixture is cooled to 100°C, add calcium stearate and continue mixing for 30 seconds, and when the mixture temperature reaches 85°C, discharge the material, crush and screen to obtain coated sand.
[0029] Example 3 A rare earth modified ceramsite coated sand for 3D printing, the preparation method comprising: 1. Take attapulgite clay powder and fly ash in a mass ratio of 3:20 and mix them thoroughly. Transfer the mixture into an extrusion granulator for granulation, and then place it in a furnace for calcination at 750℃ for 4 h to obtain spherical ceramsite with a porous structure. Weigh cerium fluoride, lanthanum oxide, and yttrium fluoride in a mass ratio of 1:0.2:0.4 as a modifier, take 100 parts of the above ceramsite and 1 part of the modifier, disperse the modifier in deionized water, add ceramsite, stir and ultrasonicate (ultrasonic power 35 W, every 5 min of ultrasound interval 1 h, 100 rpm continuous stirring for 12 h); adjust the pore size of the filter medium, separate the ceramsite and the modifier dispersion, recycle the obtained dispersion, and after the ceramsite is dried, transfer it to a muffle furnace and roast it at 1000℃ for 2 h to obtain modified ceramsite (AFS particle size 75-85).
[0030] 2. Take equal masses of yellow rosin (first grade) and soybean oil acid (saponification value 205 mg / g), heat to 130℃ and mix evenly, then add E44 bisphenol A epoxy resin which is 5 times of the total mass of the two, stir at 190℃ for 4 h, cool after the reaction, wash, filter and dry to obtain rosin-modified epoxy resin; take the obtained rosin-modified epoxy resin and rosin-modified phenolic resin 2112 (purchased from Shangrao Sinan) in a mass ratio of 10:3 to form rosin-modified resin.
[0031] 3. Weigh 120 parts of quartz sand (SiO2 content 96%, AFS particle size 60-70), 10 parts of the above modified ceramsite, 3 parts of thermoplastic phenolic resin PF-1904, 2 parts of the above rosin modified resin, 1.2 parts of urotropine (40% by mass hexamethylenetetramine aqueous solution), 1.6 parts of calcium stearate, and 0.3 parts of KH550 by weight. Mix the quartz sand and modified ceramsite thoroughly, heat to 105°C and transfer to a sand mixer; continue to add thermoplastic phenolic resin, rosin modified resin and KH550, heat to 135°C and mix for 4 minutes; when the mixture is cooled to 110°C, add urotropine to the sand mixer and mix for 1.2 minutes; when the mixture is cooled to 100°C, add calcium stearate and continue mixing for 30 seconds, and when the mixture temperature reaches 85°C, discharge the material, crush and screen to obtain coated sand.
[0032] Comparative Example 1 Refer to the step parameters of Example 1, except that the whole amount of fly ash is used to replace the attapulgite clay powder and fly ash composition in a mass ratio of 1:8 to burn the spherical ceramsite.
[0033] Comparative Example 2 The step parameters are as in Example 1, except that cerium fluoride is used alone as a modifier instead of a mixed modifier of cerium fluoride, lanthanum oxide and yttrium fluoride.
[0034] Comparative Example 3 Refer to the step parameters of Example 1, except that no ultrasonic assistance is applied during the ceramsite modification process.
[0035] Comparative Example 4 Refer to the step parameters of Example 1, except that the adhesive does not use rosin-modified epoxy resin. That is, the amount of raw materials used is: 115 parts of quartz sand (SiO2 content 96%, AFS particle size 60-70), 15 parts of modified ceramsite prepared in step 1 of Example 1, 3.5 parts of thermoplastic phenolic resin PF-1904, 1.5 parts of rosin-modified phenolic resin 2112, 1.2 parts of urotropine (40% by mass aqueous solution of hexamethylenetetramine), 1.6 parts of calcium stearate, and 0.3 parts of KH550.
[0036] Test example The performance of the coated sand samples obtained in the above Examples 1-3 and Comparative Examples 1-4 was tested (GB / T 42156-2023): the coated sand samples were placed in a laser sintering 3D printing device to make specimens, and the parameters were set as follows: laser power 25 W, scanning speed 1500 mm / s; after keeping at 250°C for 20 min, the test results are as shown in the following table.
[0037] Table 1
[0038] In summary, the coated sand samples prepared by the present invention have higher initial and room-temperature tensile strength, and at the same time, have low gas evolution, which can ensure the dimensional accuracy and surface quality of the processed castings and meet the performance requirements of 3D printed coated sand casting.
[0039] The embodiments described above only express several preferred embodiments of the present invention, and the descriptions thereof are relatively specific and detailed, but are not intended to limit the present invention. It should be noted that for those skilled in the art, the present invention may also have various changes and modifications, and any modifications, equivalent substitutions, improvements, etc. made within the concept and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A rare earth modified ceramsite coated sand for 3D printing, characterized in that: The preparation materials include the following by weight: 110-120 parts of quartz sand, 10-20 parts of modified ceramsite, 3-4.5 parts of thermoplastic phenolic resin, 1-2 parts of rosin modified resin, 1-1.4 parts of methenamine, Calcium stearate 1.2-1.8 parts, Coupling agent 0.2-0.3 parts.
2. The rare earth modified ceramsite coated sand for 3D printing according to claim 1, characterized in that: The modified ceramsite is a rare earth modified ceramsite obtained by modifying ceramsite with cerium fluoride, lanthanum oxide and yttrium fluoride; the preparation method of the rare earth modified ceramsite is as follows: cerium fluoride, lanthanum oxide and yttrium fluoride are mixed and dispersed in deionized water, ceramsite is added, stirred and ultrasonicated, and filtered; the dispersion obtained by filtration is recovered and reused, and the obtained ceramsite is dried and then transferred to a muffle furnace for roasting to obtain the rare earth modified ceramsite.
3. The rare earth modified ceramsite coated sand for 3D printing according to claim 2, characterized in that: The dosage ratio of cerium fluoride, lanthanum oxide and yttrium fluoride is 1:(0.2-0.5):0.
4.
4. The rare earth modified ceramsite coated sand for 3D printing according to claim 2, characterized in that: The calcination temperature is 800-1000° C. and the calcination time is 2-4 h.
5. The rare earth modified ceramsite coated sand for 3D printing according to claim 2, characterized in that: The preparation method of the ceramsite is as follows: attapulgite clay and fly ash are fully mixed and stirred, then the obtained mixture is transferred to an extrusion granulator for granulation, and finally calcined at 650-800° C. for 3-6 h to obtain ceramsite with a porous structure.
6. The rare earth modified ceramsite coated sand for 3D printing according to claim 1, characterized in that: The rosin-modified resin is composed of rosin-modified epoxy resin and rosin-modified phenolic resin, and the mass ratio of the two is 10:(3-5).
7. The rare earth modified ceramsite coated sand for 3D printing according to claim 6, characterized in that: The preparation method of the rosin-modified epoxy resin is as follows: taking equal masses of rosin and soybean oil acid and mixing them evenly at 120-140° C., then adding 5-6 times the total mass of epoxy resin, stirring at 170-190° C. for 4-5 h, cooling, washing, filtering and drying after the reaction is completed.
8. The method for preparing the rare earth modified ceramsite coated sand for 3D printing according to any one of claims 1 to 7, characterized in that: The steps include: Step 1: Weigh all the raw materials according to the formula, mix the quartz sand and modified ceramsite thoroughly, heat to 100-110℃ and transfer to the sand mixer; Step 2: Add thermoplastic phenolic resin, rosin modified resin and coupling agent into the sand mixer, heat to 125-145℃ and mix the sand for 3-4 minutes; Step 3: When the mixture of step 2 is cooled to 105-115°C, add hexamethylenetetramine to the sand mixer and mix for 1-1.5 minutes; Step 4: After the mixture in step 3 is cooled to 95-105°C, calcium stearate is added and the sand is mixed for 30 seconds. When the temperature of the mixture reaches 80-85°C, the material is discharged, crushed and sieved to obtain coated sand.
9. The preparation method according to claim 8, characterized in that: The quartz sand needs to be processed into a nearly spherical shape before mixing, the AFS particle size of the quartz sand is 60-70, and the AFS particle size of the modified ceramsite is 75-85.