High-speed punching method and equipment for ceramic material

By using time-shaping millisecond laser on ceramic materials, pulse waveforms of high peak power front edge and low peak power middle edge and back edge are formed, the problems of low efficiency and thermal effects in ceramic micropore processing are solved, and high efficiency and high efficiency are achieved Quality micropore processing.

CN118989667AActive Publication Date: 2024-11-22CENT SOUTH UNIV

Patent Information

Application Number
CN202411310832.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-11-22
Estimated Expiration
2044-09-20

AI Technical Summary

Technical Problem

Ceramic materials have problems in micropore processing, insufficient processing efficiency, insufficient stability, high equipment costs, and thermal effects and defects caused by high peak power lasers, which are difficult to meet the needs of industrial processing.

Method used

Millisecond pulse laser using time-shaping has specific pulse waveforms of high peak power front and low peak power medium edge and trailing edge. It forms defects on ceramic materials through high peak power front, enhances subsequent laser absorption, and utilizes low peak power medium Micropore processing is achieved along and behind edges to reduce thermal effects and thermal defects.

Benefits of technology

It realizes high efficiency and high-quality micropore processing of ceramic materials, controls micropore diameter and thermal defects, and improves processing efficiency and quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118989667A_ABST
    Figure CN118989667A_ABST
Patent Text Reader

Abstract

The invention provides a high-speed punching method and equipment for a ceramic material. The high-efficiency and high-quality micropore processing of the ceramic material is carried out by utilizing time-shaped millisecond pulse laser. Specifically, the output millisecond laser has specific pulse waveforms of a high peak power leading edge and a low peak power middle edge and a low peak power trailing edge by regulating the control of a laser; the millisecond laser firstly passes through the collimating mirror so as to have low-divergence and long-distance transmission capabilities, then deflection of the millisecond laser is controlled by the galvanometer, and finally the millisecond laser is focused by the focusing mirror and then acts on a specified position on the upper surface of a sample; the high peak power leading edge of the millisecond laser acts on a sample to generate a defect, and the defect can significantly increase the absorption of the ceramic material to the subsequent millisecond laser, so that the subsequent low peak power middle edge and trailing edge can form required micropore processing under absorption enhancement, the thermal effect of millisecond laser processing is reduced, the micropore diameter, the thermal defect and the like are controlled, and the quality of the product is improved. And high-efficiency and high-quality micropore processing of the ceramic material is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of laser processing, and in particular to a high-speed drilling method and equipment for ceramic materials. Background Art

[0002] Ceramics have the characteristics of high hardness, thermal conductivity, resistivity, thermal stability, small dielectric constant, and thermal expansion coefficient matching the chip. They are the first choice for the new generation of microelectronic devices and systems. They have become the main material for circuit substrates in aerospace, 5G communications, high-power power semiconductors, and high-power LED lighting, and have broad application prospects. However, ceramics are typical hard and brittle materials, and traditional mechanical processing can easily lead to substrate fracture, and special processing methods are also greatly limited. With the maturity of industrial laser technology and the popularization of its application, laser processing, as a new non-contact, wear-free green technology, has become a new choice for ceramic circuit substrate processing with high precision, high efficiency, and controllable process.

[0003] In existing research, the rapid development of nanosecond, picosecond, and femtosecond lasers has enabled them to demonstrate significant quality advantages in micron and nanometer manufacturing. However, the current status of low processing efficiency, insufficient stability, and expensive equipment costs makes it difficult to meet the needs of industrial processing of ceramic substrates. Millisecond lasers with large pulse energy have high material removal efficiency, but processing is accompanied by obvious thermal effects, the sputtering of molten ceramics is insufficient, and micropores are often accompanied by defects such as large apertures, large tapers, and microcracks. Therefore, how to achieve high-efficiency and high-quality micropore processing of ceramic materials has become a problem that needs to be solved urgently.

[0004] Ceramic materials have very low absorption of lasers. For example, alumina ceramics generally absorb less than 5% of near-infrared lasers. Therefore, traditional millisecond lasers often require extremely high peak power density to form a certain ablation effect on the ceramic surface during micro-hole processing of ceramic materials. However, there will be a sudden increase in absorption rate during the entire cycle of this type of high-peak power density millisecond laser drilling: after the millisecond laser ablation forms a defective small hole on the initial surface, the subsequently injected high-peak power pulse laser will be effectively absorbed by the multiple reflections of the smooth inner wall of the small hole. The small hole of appropriate depth can even increase the absorption of the millisecond laser to saturation (similar to a black hole). Therefore, in the later stage of millisecond laser processing of ceramic micro-holes, the material heated, melted and vaporized by the millisecond laser will increase significantly due to the increased absorption, resulting in the expansion of the micro-hole diameter and the increase of thermal defects (cracks, recast layer thickness, micro-hole taper, etc.), which is difficult to meet actual needs.

[0005] In response to the above problems, this patent proposes a new high-speed drilling method and equipment for ceramic materials, which specifically uses a time-shaped millisecond pulse laser to perform micro-hole processing on ceramic materials, wherein the time-shaped millisecond laser has a high-peak power front edge and a low-peak power middle edge and trailing edge, and fully utilizes the high-peak power front edge to prepare defects on the ceramic material. The defect will significantly increase the ceramic material's absorption of subsequent millisecond lasers, so that the subsequent low-peak power middle edge and trailing edge can form the desired micro-hole processing under enhanced absorption, reducing the thermal effect of millisecond laser processing, thereby controlling the micro-hole diameter, thermal defects, etc. Summary of the invention

[0006] The present invention provides a novel high-speed ceramic material drilling method and equipment, comprising the following steps:

[0007] Step 1: by adjusting the control of the laser, the output millisecond laser has a specific pulse waveform with a high peak power leading edge and a low peak power middle edge and trailing edge;

[0008] Step 2: The laser passes through a collimator to have low divergence and long-distance transmission capabilities, and then its deflection is controlled by a galvanometer, and then focused by a focusing mirror to act on a specified position on the upper surface of the sample;

[0009] Step 3. The high peak power front edge of the millisecond pulse laser acts on the sample to produce defects. The defects will significantly increase the sample's absorption of subsequent millisecond lasers. Therefore, the low peak power middle edge and trailing edge can achieve the required micro-hole processing, effectively reduce the thermal effect during the processing, and ultimately achieve high-efficiency and high-quality micro-hole processing of ceramic materials.

[0010] Furthermore, the wavelength of the millisecond laser is in the range of 266-2000 nm.

[0011] Furthermore, the method of regulating the waveform of the millisecond laser pulse includes but is not limited to controlling the waveform of the laser input excitation.

[0012] Furthermore, the peak power of the leading edge of the millisecond laser pulse is more than three times the peak power of the middle edge and the trailing edge.

[0013] Furthermore, the front edge pulse width of the millisecond laser pulse is 50μs-1ms, the peak power is 3kW-15kW, the middle edge and trailing edge pulse width of the millisecond laser pulse is 100μs-10ms, and the peak power is 1kW-3kW.

[0014] Furthermore, the defect has a diameter of 5 μm-100 μm, a depth of 1 μm-20 μm, and a shape of cone, flat top, etc. The defect can increase the material absorption by more than 5 times.

[0015] Furthermore, the sample is made of materials such as aluminum oxide, aluminum nitride, and silicon nitride.

[0016] Furthermore, the thickness of the sample is 0.2 mm-5 mm.

[0017] Furthermore, the galvanometer adjusts the direction of the laser so that it is incident perpendicularly on the sample surface, and controls the processing path of the laser on the sample by moving the galvanometer.

[0018] Furthermore, the sample is fixed by a fixture and a stage, and its upper surface is located at the laser focus position.

[0019] Beneficial Effects

[0020] The present invention mainly has the following technical advantages:

[0021] 1. By forming a specific pulse waveform (with a high peak power front edge, a low peak power middle edge, and a trailing edge), the problem of absorptivity change during the millisecond laser drilling process of ceramic materials is solved, and the pulse front edge is fully utilized to prepare defects on the ceramic surface to enhance laser absorption, thereby reducing the overall injected laser energy and the thermal effect of millisecond laser processing, thereby controlling the micropore diameter, thermal defects, etc., and improving the quality of the micropores.

[0022] 2. Since defects greatly increase the absorption of subsequent lasers, the required through-holes can be formed under the action of a single pulse through a suitable waveform, and can be applied to high-speed movement and scanning drilling, thereby improving processing efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The millisecond laser output timing diagram of the ceramic material high-speed drilling method and equipment provided by the present invention shows a typical laser waveform of a high-peak power leading edge and a low-peak power middle edge and trailing edge.

[0024] Specifically, the peak power of the pulse front is much greater than the peak power of the pulse middle and trailing edges (more than 3 times), while the width of the pulse front is much smaller than the width of the pulse middle and trailing edges, thereby satisfying the requirements of pulse front manufacturing defects and stable absorption of the pulse middle and trailing edges.

[0025] Figure 2 A schematic diagram of the technical solution of the high-speed drilling method and equipment for ceramic materials provided by the present invention.

[0026] [Description of Reference Numerals]

[0027] 1. Time-shaped millisecond laser; 2. Collimating mirror; 3. Galvanometer; 4. Focusing mirror; 5. Laser focus; 6. Ceramic material. DETAILED DESCRIPTION

[0028] In order to make the technical problems, technical solutions and advantages to be solved by the present invention clearer, the following will be described in detail with reference to the accompanying drawings and specific embodiments. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention.

[0029] Example 1

[0030] Alumina ceramic pieces of 30mm×30mm×1mm were selected as samples. The millisecond laser was controlled to output millisecond lasers with high peak power front edge and low peak power middle edge and trailing edge waveforms, the laser wavelength was 1030nm, the repetition frequency was 100Hz, the peak power of the pulse front edge was 15kW, the front edge width was 1ms, the peak power of the pulse middle edge and trailing edge was 5kW, and the middle edge and trailing edge width were 3ms.

[0031] After passing through the collimator 2, the laser has low divergence and long-distance transmission capabilities. After being deflected by the galvanometer 3, it is focused by the focusing mirror 4 and acts on the specified position 5 on the upper surface of the sample 6. The high peak power front edge of the millisecond pulse laser acts on the sample to produce defects, which significantly increase the sample's absorption of subsequent millisecond lasers. Therefore, the low peak power middle edge and trailing edge can achieve the required micro-hole processing, and the thermal effect is effectively reduced.

[0032] This embodiment adopts single pulse scanning drilling, each pulse directly processes a microhole, and the laser is controlled by the movement of the galvanometer to continuously process the microholes on the sample, ultimately achieving high-efficiency and high-quality microhole processing.

[0033] Example 2

[0034] A 20mm×10mm×2mm silicon nitride ceramic sheet was selected as the sample. The millisecond laser was controlled to output a millisecond laser with a high peak power front edge and a low peak power middle edge and trailing edge waveform, the laser wavelength was 1080nm, the repetition frequency was 20Hz, the peak power of the pulse front edge was 12kW, the front edge width was 500μs, the peak power of the pulse middle edge and trailing edge was 3kW, and the middle edge and trailing edge width was 4ms.

[0035] After passing through the collimator 2, the laser has low divergence and long-distance transmission capabilities. After being deflected by the galvanometer 3, the laser is focused by the focusing mirror 4 and acts on the specified position 5 on the upper surface of the sample 6. In this embodiment, one microhole is processed under the action of every five laser pulses. Similarly, the processing path of the laser is controlled by the movement of the galvanometer to achieve high-efficiency and high-quality microhole processing.

[0036] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method and equipment for high-speed drilling of ceramic materials, characterized in that: include: Step 1: by adjusting the control of the laser, the output millisecond laser has a specific pulse waveform with a high peak power leading edge and a low peak power middle edge and trailing edge; Step 2: The laser passes through a collimator to have low divergence and long-distance transmission capabilities, and then its deflection is controlled by a galvanometer, and then focused by a focusing mirror to act on a specified position on the upper surface of the sample; Step 3. The high peak power front edge of the millisecond pulse laser acts on the sample to produce defects. The defects will significantly increase the sample's absorption of subsequent millisecond lasers. Therefore, the low peak power middle edge and trailing edge can achieve the required micro-hole processing, effectively reduce the thermal effect during the processing, and ultimately achieve high-efficiency and high-quality micro-hole processing of ceramic materials.

2. The high-speed drilling method and equipment for ceramic materials according to claim 1, characterized in that: The wavelength of the millisecond laser is in the range of 266-2000 nm.

3. The high-speed drilling method and equipment for ceramic materials according to claim 1, characterized in that: Ways to regulate the waveform of the millisecond laser pulse include, but are not limited to, controlling the waveform of the laser input excitation.

4. The high-speed drilling method and equipment for ceramic materials according to claim 1, characterized in that: The peak power of the front edge of the millisecond laser pulse is more than three times the peak power of the middle edge and the rear edge.

5. The high-speed drilling method and equipment for ceramic materials according to claim 1, characterized in that: The front edge pulse width of the millisecond laser pulse is 50μs-1ms, the peak power is 3kW-15kW, the middle edge and rear edge pulse width of the millisecond laser pulse are 100μs-10ms, and the peak power is 1kW-3kW.

6. The high-speed drilling method and equipment for ceramic materials according to claim 1, characterized in that: The defect has a diameter of 5 μm-100 μm, a depth of 1 μm-20 μm, and a shape of cone, flat top, etc. The defect can increase the material absorption by more than 5 times.

7. The high-speed drilling method and equipment for ceramic materials according to claim 1, characterized in that: The samples are made of materials such as aluminum oxide, aluminum nitride, and silicon nitride.

8. The high-speed drilling method and equipment for ceramic materials according to claim 1, characterized in that: The thickness of the sample is 0.2 mm-5 mm.

9. The high-speed drilling method and equipment for ceramic materials according to claim 1, characterized in that: The galvanometer adjusts the direction of the laser so that it is incident perpendicularly on the sample surface, and controls the processing path of the laser on the sample by moving the galvanometer.

10. The high-speed drilling method and equipment for ceramic materials according to claim 1, characterized in that: The sample is fixed by a fixture and a stage, and its upper surface is located at the laser focus position.

Citation Information

Patent Citations

  • Pulsed laser machining method and installation, particularly for welding, with variation of the power of each laser pulse

    CN103108721A

  • Method for processing micropore with large depth-diameter ratio through ultrafast laser

    CN117862704A

  • Micromachining with high-energy, intra-cavity Q-switched CO2 laser pulses

    US20020185474A1

  • System for and method of zoom processing

    US20060000816A1

  • Simulation system and method for laser drilling process

    WO2015113302A1

Cited By

  • Laser cutting method, device and system and ultrafast pulse laser

    CN119282441A