High-strength bolt used on subway and machining method of high-strength bolt

By combining specific elements and processing techniques, the strength and rust resistance of high-strength bolts used in subways are improved, solving the problem of bolts being prone to rusting in humid environments and enabling efficient use under humid conditions.

CN118989867APending Publication Date: 2024-11-22NANJING HI-RAIL TRANS TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411062754.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The high-strength bolts currently used in subways are prone to rusting in humid environments, causing inconvenience in use and resulting in lower strength.

Method used

A zinc coating is formed by combining carbon, manganese, chromium, molybdenum, nickel, silicon, titanium, sulfur and zinc in a specific ratio, through hot melting and mixing, cold forging, heat treatment, threading and surface treatment, which improves the strength and corrosion resistance of the bolts.

Benefits of technology

It significantly improves the strength and durability of bolts, making them suitable for use in humid and corrosive climates and extending their service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118989867A_ABST
    Figure CN118989867A_ABST
Patent Text Reader

Abstract

The invention discloses a high-strength bolt used on a subway and a processing method thereof, the high-strength bolt comprises the following raw materials: 1-30 parts of carbon, 1-25 parts of manganese, 1-22 parts of chromium, 1-20 parts of molybdenum, 1-15 parts of nickel, 1-15 parts of silicon, 1-10 parts of titanium, 1-8 parts of sulfur and 1-5 parts of zinc, and the processing method comprises the following steps: S1, hot melting mixing; s2, cold forging forming; s3, heat treatment; s4, thread machining; s5, surface treatment; and S6, quality inspection is conducted, in the step S1, carbon, manganese, sulfur, chromium, molybdenum, nickel, silicon, titanium and sulfur are put into a vacuum furnace, the temperature of the vacuum furnace is 600-800 DEG C, preheating is conducted for 10-30 min, then the vacuum furnace is heated to 1500-2000 DEG C, heating is conducted for 10-20 min, finally air cooling is conducted to the room temperature, and a blank is prepared. Through cooperation of all the elements, the strength and the anti-rust effect of the high-strength bolt are effectively improved, the durability of a high-strength bolt product is greatly improved, the performance of the high-strength bolt is improved, and the high-strength bolt has good practicability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of bolts, and in particular to a high-strength bolt used in subways and a processing method thereof. Background Art

[0002] Bolt: A mechanical part, a cylindrical threaded fastener with a nut. A type of fastener consisting of a head and a screw, a cylindrical body with external threads, which must be matched with a nut to fasten two parts with through holes. This type of connection is called a bolt connection. If the nut is unscrewed from the bolt, the two parts can be separated, so the bolt connection is a detachable connection. High-strength bolts are usually used in structures that need to withstand large tension and loads, such as bridges, building structures, mechanical equipment, etc. Their characteristics include high material strength, good corrosion resistance, and stable performance in extreme environments.

[0003] The invention with the announcement number: CN109881111A discloses a high-strength bolt, which is composed of the following chemical components in weight percentage: Cr: 0.93-1.45%; Mn: 0.35-0.95%; C: 0.32-0.41%; Ni: 0.15-0.35%; Cu: 0.12-0.22%; Mo: 0.09-0.24%; S: 0.08-0.18%; Al: 0.06-0.12%; N: ≤0.065%; S: ≤0.028%; P: ≤0.023%; Ti: ≤0.021%; Ce: ≤0.018%; O: ≤0.002%, and the rest is Fe and unavoidable impurities. The manufacturing method of the high-strength bolt is also disclosed. The present invention improves the traditional process, changes the component ratio of the bolt raw materials, and further optimizes the content of each component, so that the comprehensive performance of the bolt is improved.

[0004] The invention with announcement number: CN105506496A discloses a method for making high-strength prestressed bolts, that is, the method adopts vacuum induction and electroslag remelting process to smelt medium carbon alloy steel, and controls the impurity content; adopts vacuum furnace for heat treatment, quenching temperature is 860°C, first high temperature tempering temperature is 560°C, and second tempering temperature is 500°C; according to the required bolt specifications, machining is performed, the thread is processed by thread rolling, the middle diameter tolerance is controlled within 0.1mm, the surface roughness of the bolt and the thread roughness are Ra0.8, and all transition positions of the bolt adopt arc transition greater than R20. The bolts made by this method have the advantages of high strength and high toughness, and their mechanical property detection indicators meet the tightening of components subjected to large alternating loads, ensuring the safe and reliable operation of the components, and reducing the production cost and cycle.

[0005] The high-strength bolts used on subways in the prior art have low strength in actual use, and the underground is relatively humid, which easily causes the bolts to rust, resulting in inconvenience in use. Therefore, the present invention proposes a high-strength bolt used in subways and a processing method thereof to solve the above problems. Summary of the invention

[0006] Based on the technical problem that in actual use, the strength of the bolts is low and the underground is relatively humid, which easily causes the bolts to rust and causes inconvenience in use, the present invention proposes a high-strength bolt for use on a subway and a processing method thereof.

[0007] The invention provides a high-strength bolt for use on a subway, comprising the following raw materials: 1-30 parts of carbon, 1-25 parts of manganese, 1-22 parts of chromium, 1-20 parts of molybdenum, 1-15 parts of nickel, 1-15 parts of silicon, 1-10 parts of titanium, 1-8 parts of sulfur and 1-5 parts of zinc.

[0008] Through the above mechanism: manganese can significantly improve the hardness, strength and wear resistance of steel, chromium can increase the corrosion resistance and wear resistance of steel, molybdenum can improve the hardness, corrosion resistance and high temperature resistance of steel, nickel can be added to steel to improve its corrosion resistance and high temperature resistance, silicon can improve the hardness, heat resistance and chemical stability of steel when used, titanium has very high strength and excellent corrosion resistance, and at the same time has a relatively low density. Through the combination of the above elements, the strength of high-strength bolts is greatly enhanced. Through the excellent corrosion resistance of titanium, it has high resistance to harmful environments, thereby enhancing the durability of high-strength bolts. By melting zinc and then immersing the high-strength bolts in molten zinc, a uniform zinc coating can be formed on the surface of the high-strength bolts. The zinc coating provides a higher corrosion resistance for the high-strength bolts, making the high-strength bolts suitable for use in humid and corrosive climate conditions.

[0009] The present invention also proposes a method for processing high-strength bolts used in subways, comprising the following steps: S1: hot melt mixing; S2: cold forging; S3: heat treatment; S4: thread processing; S5: surface treatment; S6: Quality inspection.

[0010] Preferably, in the step S1, carbon, manganese, sulfur, chromium, molybdenum, nickel, silicon, titanium and sulfur are placed in a vacuum furnace with a temperature of 600-800 degrees Celsius, preheated for 10-30 minutes, then the vacuum furnace is heated to 1500-2000 degrees Celsius, heated for 10-20 minutes, and finally air-cooled to room temperature to obtain a blank.

[0011] Furthermore, the metal raw materials are first heated by preheating, and then the metal raw materials are melted together by high temperature for subsequent processing.

[0012] Preferably, in the step S2, the blank is placed in a cold heading machine and forged to obtain a bolt blank.

[0013] Furthermore, a certain pressure is applied to the metal blank by the cold heading machine, so that the metal blank undergoes plastic deformation in the die cavity and is formed into a specified shape and size.

[0014] Preferably, in the step S3, the rough bolt blank is heated at 700-850 degrees Celsius for 10-30 minutes, and then heated at 400-500 degrees Celsius for 30-60 minutes.

[0015] Furthermore, by heat treatment, without changing the shape and overall chemical composition of the workpiece, the internal microstructure of the workpiece or the chemical composition of the workpiece surface is changed, thereby imparting or improving the performance of the workpiece, improving the intrinsic quality of the bolt rough blank, and providing the bolt rough blank with the required mechanical properties, physical properties and chemical properties.

[0016] Preferably, in the step S4, the processed bolt rough blank is turned by a lathe, a thread groove is formed on the bolt rough blank, and then the head of the bolt rough blank is turned to obtain a bolt.

[0017] Furthermore, the thread groove is opened and processed on the rough bolt blank by turning. This method has the advantages of high precision and high finish, which greatly improves the production quality of the bolt.

[0018] Preferably, in the step S5, the treated high-strength bolts are immersed in molten zinc to form a uniform zinc coating to obtain high-strength bolts.

[0019] Furthermore, the zinc coating provides the high-strength bolts with a higher corrosion resistance, making the high-strength bolts suitable for use in wet and corrosive climate conditions.

[0020] Preferably, in the step S6, the size, dimensions and thread groove dimensions of the high-strength bolt are inspected, and finally the high-strength bolt is manufactured.

[0021] Beneficial effects of the present invention: The present invention effectively improves the strength and rust prevention effect of the high-strength bolt through the synergy between various elements, greatly improves the durability of the high-strength bolt products, improves the performance of the high-strength bolt, and has good practicality. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1The working flow chart proposed by the present invention. DETAILED DESCRIPTION

[0023] The present invention will be further explained below in conjunction with specific embodiments.

[0024] Reference Figure 1 , Embodiment 1 This embodiment provides a high-strength bolt for use in subways, comprising the following raw materials: 25 parts of carbon, 15 parts of manganese, 12 parts of chromium, 12 parts of molybdenum, 10 parts of nickel, 8 parts of silicon, 10 parts of titanium, 6 parts of sulfur and 2 parts of zinc.

[0025] Through the above mechanism: manganese can significantly improve the hardness, strength and wear resistance of steel, chromium can increase the corrosion resistance and wear resistance of steel, molybdenum can improve the hardness, corrosion resistance and high temperature resistance of steel, nickel can be added to steel to improve its corrosion resistance and high temperature resistance, silicon can improve the hardness, heat resistance and chemical stability of steel when used, titanium has very high strength and excellent corrosion resistance, and at the same time has a relatively low density. Through the combination of the above elements, the strength of high-strength bolts is greatly enhanced. Through the excellent corrosion resistance of titanium, it has high resistance to harmful environments, thereby enhancing the durability of high-strength bolts. By melting zinc and then immersing the high-strength bolts in molten zinc, a uniform zinc coating can be formed on the surface of the high-strength bolts. The zinc coating provides a higher corrosion resistance for the high-strength bolts, making the high-strength bolts suitable for use in humid and corrosive climate conditions.

[0026] The present invention also proposes a method for processing high-strength bolts used in subways, comprising the following steps: S1: hot melt mixing; S2: cold forging; S3: heat treatment; S4: thread processing; S5: surface treatment; S6: Quality inspection.

[0027] Preferably, in the step S1, carbon, manganese, sulfur, chromium, molybdenum, nickel, silicon, titanium and sulfur are placed in a vacuum furnace with a temperature of 700 degrees Celsius and preheated for 18 minutes. The vacuum furnace is then heated to 1800 degrees Celsius for 15 minutes and finally air-cooled to room temperature to obtain a blank. The metal raw materials are first heated by preheating and then melted by high temperature for subsequent processing.

[0028] Preferably, in the step S2, the blank is placed in a cold heading machine and forged to obtain a bolt blank. A certain pressure is applied to the metal blank by the cold heading machine to cause the metal blank to undergo plastic deformation in the die cavity and be formed into a specified shape and size.

[0029] Preferably, in the step S3, the rough bolt blank is heated at 750 degrees Celsius for 20 minutes and then heated at 450 degrees Celsius for 50 minutes. By heat treatment, the microstructure inside the workpiece or the chemical composition on the surface of the workpiece is changed without changing the shape and overall chemical composition of the workpiece, so as to impart or improve the performance of the workpiece, improve the intrinsic quality of the rough bolt blank, and provide the rough bolt blank with the required mechanical properties, physical properties and chemical properties.

[0030] Preferably, in the step S4, the processed bolt rough blank is turned by a lathe to open a thread groove on the bolt rough blank, and then the head of the bolt rough blank is turned to obtain the bolt. The bolt rough blank is opened and processed by turning the thread groove. This method has the advantages of high precision and high finish, and greatly improves the production quality of the bolt.

[0031] Preferably, in the step S5, the treated high-strength bolts are immersed in molten zinc to form a uniform zinc coating to obtain high-strength bolts. The zinc coating provides the high-strength bolts with a higher corrosion resistance, making the high-strength bolts suitable for use in humid and corrosive climate conditions.

[0032] Preferably, in the step S6, the size, dimensions and thread groove dimensions of the high-strength bolt are inspected, and finally the high-strength bolt is manufactured.

[0033] Reference Figure 1 , Embodiment 2 This embodiment provides a high-strength bolt for use in subways, comprising the following raw materials: 22 parts of carbon, 18 parts of manganese, 15 parts of chromium, 15 parts of molybdenum, 12 parts of nickel, 6 parts of silicon, 7 parts of titanium, 4 parts of sulfur and 1 part of zinc.

[0034] Through the above mechanism: manganese can significantly improve the hardness, strength and wear resistance of steel, chromium can increase the corrosion resistance and wear resistance of steel, molybdenum can improve the hardness, corrosion resistance and high temperature resistance of steel, nickel can be added to steel to improve its corrosion resistance and high temperature resistance, silicon can improve the hardness, heat resistance and chemical stability of steel when used, titanium has very high strength and excellent corrosion resistance, and at the same time has a relatively low density. Through the combination of the above elements, the strength of high-strength bolts is greatly enhanced. Through the excellent corrosion resistance of titanium, it has high resistance to harmful environments, thereby enhancing the durability of high-strength bolts. By melting zinc and then immersing the high-strength bolts in molten zinc, a uniform zinc coating can be formed on the surface of the high-strength bolts. The zinc coating provides a higher corrosion resistance for the high-strength bolts, making the high-strength bolts suitable for use in humid and corrosive climate conditions.

[0035] The present invention also proposes a method for processing high-strength bolts used in subways, comprising the following steps: S1: hot melt mixing; S2: cold forging; S3: heat treatment; S4: thread processing; S5: surface treatment; S6: Quality inspection.

[0036] Preferably, in the step S1, carbon, manganese, sulfur, chromium, molybdenum, nickel, silicon, titanium and sulfur are placed in a vacuum furnace with a temperature of 750 degrees Celsius and preheated for 20 minutes. The vacuum furnace is then heated to 1850 degrees Celsius for 20 minutes and finally air-cooled to room temperature to obtain a blank. The metal raw materials are first heated by preheating and then melted into one by high temperature for subsequent processing.

[0037] Preferably, in the step S2, the blank is placed in a cold heading machine and forged to obtain a bolt blank. A certain pressure is applied to the metal blank by the cold heading machine to cause the metal blank to undergo plastic deformation in the die cavity and be formed into a specified shape and size.

[0038] Preferably, in the step S3, the rough bolt blank is heated at 800 degrees Celsius for 18 minutes and then heated at 450 degrees Celsius for 60 minutes. By heat treatment, the microstructure inside the workpiece or the chemical composition on the surface of the workpiece is changed without changing the shape and overall chemical composition of the workpiece, so as to impart or improve the performance of the workpiece, improve the intrinsic quality of the rough bolt blank, and provide the rough bolt blank with the required mechanical properties, physical properties and chemical properties.

[0039] Preferably, in the step S4, the processed bolt rough blank is turned by a lathe to open a thread groove on the bolt rough blank, and then the head of the bolt rough blank is turned to obtain the bolt. The bolt rough blank is opened and processed by turning the thread groove. This method has the advantages of high precision and high finish, and greatly improves the production quality of the bolt.

[0040] Preferably, in the step S5, the treated high-strength bolts are immersed in molten zinc to form a uniform zinc coating to obtain high-strength bolts. The zinc coating provides the high-strength bolts with a higher corrosion resistance, making the high-strength bolts suitable for use in humid and corrosive climate conditions.

[0041] Preferably, in the step S6, the size, dimensions and thread groove dimensions of the high-strength bolt are inspected, and finally the high-strength bolt is manufactured.

[0042] Reference Figure 1 , Embodiment 3 This embodiment provides a high-strength bolt for use in subways, comprising the following raw materials: 28 parts of carbon, 16 parts of manganese, 18 parts of chromium, 17 parts of molybdenum, 9 parts of nickel, 3 parts of silicon, 4 parts of titanium, 4 parts of sulfur and 1 part of zinc.

[0043] Through the above mechanism: manganese can significantly improve the hardness, strength and wear resistance of steel, chromium can increase the corrosion resistance and wear resistance of steel, molybdenum can improve the hardness, corrosion resistance and high temperature resistance of steel, nickel can be added to steel to improve its corrosion resistance and high temperature resistance, silicon can improve the hardness, heat resistance and chemical stability of steel when used, titanium has very high strength and excellent corrosion resistance, and at the same time has a relatively low density. Through the combination of the above elements, the strength of high-strength bolts is greatly enhanced. Through the excellent corrosion resistance of titanium, it has high resistance to harmful environments, thereby enhancing the durability of high-strength bolts. By melting zinc and then immersing the high-strength bolts in molten zinc, a uniform zinc coating can be formed on the surface of the high-strength bolts. The zinc coating provides a higher corrosion resistance for the high-strength bolts, making the high-strength bolts suitable for use in humid and corrosive climate conditions.

[0044] The present invention also proposes a method for processing high-strength bolts used in subways, comprising the following steps: S1: hot melt mixing; S2: cold forging; S3: heat treatment; S4: thread processing; S5: surface treatment; S6: Quality inspection.

[0045] Preferably, in the step S1, carbon, manganese, sulfur, chromium, molybdenum, nickel, silicon, titanium and sulfur are placed in a vacuum furnace with a temperature of 650 degrees Celsius and preheated for 20 minutes. The vacuum furnace is then heated to 1600 degrees Celsius for 16 minutes and finally air-cooled to room temperature to obtain a blank. The metal raw materials are first heated by preheating and then melted into one by high temperature for subsequent processing.

[0046] Preferably, in the step S2, the blank is placed in a cold heading machine and forged to obtain a bolt blank. A certain pressure is applied to the metal blank by the cold heading machine to cause the metal blank to undergo plastic deformation in the die cavity and be formed into a specified shape and size.

[0047] Preferably, in the step S3, the rough bolt blank is heated at 800 degrees Celsius for 25 minutes and then heated at 500 degrees Celsius for 50 minutes. By heat treatment, the microstructure inside the workpiece or the chemical composition on the surface of the workpiece is changed without changing the shape and overall chemical composition of the workpiece, so as to impart or improve the performance of the workpiece, improve the intrinsic quality of the rough bolt blank, and provide the rough bolt blank with the required mechanical properties, physical properties and chemical properties.

[0048] Preferably, in the step S4, the processed bolt rough blank is turned by a lathe to open a thread groove on the bolt rough blank, and then the head of the bolt rough blank is turned to obtain the bolt. The bolt rough blank is opened and processed by turning the thread groove. This method has the advantages of high precision and high finish, and greatly improves the production quality of the bolt.

[0049] Preferably, in the step S5, the treated high-strength bolts are immersed in molten zinc to form a uniform zinc coating to obtain high-strength bolts. The zinc coating provides the high-strength bolts with a higher corrosion resistance, making the high-strength bolts suitable for use in humid and corrosive climate conditions.

[0050] Preferably, in the step S6, the size, dimensions and thread groove dimensions of the high-strength bolt are inspected, and finally the high-strength bolt is manufactured.

[0051] Reference Figure 1 , Embodiment 4 This embodiment provides a high-strength bolt for use in subways, comprising the following raw materials: 20 parts of carbon, 24 parts of manganese, 18 parts of chromium, 11 parts of molybdenum, 6 parts of nickel, 5 parts of silicon, 8 parts of titanium, 4 parts of sulfur and 4 parts of zinc.

[0052] Through the above mechanism: manganese can significantly improve the hardness, strength and wear resistance of steel, chromium can increase the corrosion resistance and wear resistance of steel, molybdenum can improve the hardness, corrosion resistance and high temperature resistance of steel, nickel can be added to steel to improve its corrosion resistance and high temperature resistance, silicon can improve the hardness, heat resistance and chemical stability of steel when used, titanium has very high strength and excellent corrosion resistance, and at the same time has a relatively low density. Through the combination of the above elements, the strength of high-strength bolts is greatly enhanced. Through the excellent corrosion resistance of titanium, it has high resistance to harmful environments, thereby enhancing the durability of high-strength bolts. By melting zinc and then immersing the high-strength bolts in molten zinc, a uniform zinc coating can be formed on the surface of the high-strength bolts. The zinc coating provides a higher corrosion resistance for the high-strength bolts, making the high-strength bolts suitable for use in humid and corrosive climate conditions.

[0053] The present invention also proposes a method for processing high-strength bolts used in subways, comprising the following steps: S1: hot melt mixing; S2: cold forging; S3: heat treatment; S4: thread processing; S5: surface treatment; S6: Quality inspection.

[0054] Preferably, in the step S1, carbon, manganese, sulfur, chromium, molybdenum, nickel, silicon, titanium and sulfur are placed in a vacuum furnace with a temperature of 700 degrees Celsius and preheated for 30 minutes. The vacuum furnace is then heated to 1650 degrees Celsius for 20 minutes and finally air-cooled to room temperature to obtain a blank. The metal raw materials are first heated by preheating and then melted into one by high temperature for subsequent processing.

[0055] Preferably, in the step S2, the blank is placed in a cold heading machine and forged to obtain a bolt blank. A certain pressure is applied to the metal blank by the cold heading machine to cause the metal blank to undergo plastic deformation in the die cavity and be formed into a specified shape and size.

[0056] Preferably, in the step S3, the rough bolt blank is heated at 700 degrees Celsius for 15 minutes and then heated at 400 degrees Celsius for 40 minutes. By heat treatment, the microstructure inside the workpiece or the chemical composition on the surface of the workpiece is changed without changing the shape and overall chemical composition of the workpiece, so as to impart or improve the performance of the workpiece, improve the intrinsic quality of the rough bolt blank, and provide the rough bolt blank with the required mechanical properties, physical properties and chemical properties.

[0057] Preferably, in the step S4, the processed bolt rough blank is turned by a lathe to open a thread groove on the bolt rough blank, and then the head of the bolt rough blank is turned to obtain the bolt. The bolt rough blank is opened and processed by turning the thread groove. This method has the advantages of high precision and high finish, and greatly improves the production quality of the bolt.

[0058] Preferably, in the step S5, the treated high-strength bolts are immersed in molten zinc to form a uniform zinc coating to obtain high-strength bolts. The zinc coating provides the high-strength bolts with a higher corrosion resistance, making the high-strength bolts suitable for use in humid and corrosive climate conditions.

[0059] Preferably, in the step S6, the size, dimensions and thread groove dimensions of the high-strength bolt are inspected, and finally the high-strength bolt is manufactured.

[0060] Reference Figure 1 Embodiment 5 This embodiment provides a high-strength bolt for use in subways, comprising the following raw materials: 27 parts of carbon, 20 parts of manganese, 12 parts of chromium, 14 parts of molybdenum, 12 parts of nickel, 7 parts of silicon, 3 parts of titanium, 4 parts of sulfur and 1 part of zinc.

[0061] Through the above mechanism: manganese can significantly improve the hardness, strength and wear resistance of steel, chromium can increase the corrosion resistance and wear resistance of steel, molybdenum can improve the hardness, corrosion resistance and high temperature resistance of steel, nickel can be added to steel to improve its corrosion resistance and high temperature resistance, silicon can improve the hardness, heat resistance and chemical stability of steel when used, titanium has very high strength and excellent corrosion resistance, and at the same time has a relatively low density. Through the combination of the above elements, the strength of high-strength bolts is greatly enhanced. Through the excellent corrosion resistance of titanium, it has high resistance to harmful environments, thereby enhancing the durability of high-strength bolts. By melting zinc and then immersing the high-strength bolts in molten zinc, a uniform zinc coating can be formed on the surface of the high-strength bolts. The zinc coating provides a higher corrosion resistance for the high-strength bolts, making the high-strength bolts suitable for use in humid and corrosive climate conditions.

[0062] The present invention also proposes a method for processing high-strength bolts used in subways, comprising the following steps: S1: hot melt mixing; S2: cold forging; S3: heat treatment; S4: thread processing; S5: surface treatment; S6: Quality inspection.

[0063] Preferably, in the step S1, carbon, manganese, sulfur, chromium, molybdenum, nickel, silicon, titanium and sulfur are placed in a vacuum furnace with a temperature of 600 degrees Celsius and preheated for 30 minutes. The vacuum furnace is then heated to 1700 degrees Celsius for 20 minutes and finally air-cooled to room temperature to obtain a blank. The metal raw materials are first heated by preheating and then melted into one by high temperature for subsequent processing.

[0064] Preferably, in the step S2, the blank is placed in a cold heading machine and forged to obtain a bolt blank. A certain pressure is applied to the metal blank by the cold heading machine to cause the metal blank to undergo plastic deformation in the die cavity and be formed into a specified shape and size.

[0065] Preferably, in the step S3, the rough bolt blank is heated at 700 degrees Celsius for 30 minutes and then heated at 400 degrees Celsius for 60 minutes. By heat treatment, the microstructure inside the workpiece or the chemical composition on the surface of the workpiece is changed without changing the shape and overall chemical composition of the workpiece, so as to impart or improve the performance of the workpiece, improve the intrinsic quality of the rough bolt blank, and provide the rough bolt blank with the required mechanical properties, physical properties and chemical properties.

[0066] Preferably, in the step S4, the processed bolt rough blank is turned by a lathe to open a thread groove on the bolt rough blank, and then the head of the bolt rough blank is turned to obtain the bolt. The bolt rough blank is opened and processed by turning the thread groove. This method has the advantages of high precision and high finish, and greatly improves the production quality of the bolt.

[0067] Preferably, in the step S5, the treated high-strength bolts are immersed in molten zinc to form a uniform zinc coating to obtain high-strength bolts. The zinc coating provides the high-strength bolts with a higher corrosion resistance, making the high-strength bolts suitable for use in humid and corrosive climate conditions.

[0068] Preferably, in the step S6, the size, dimensions and thread groove dimensions of the high-strength bolt are inspected, and finally the high-strength bolt is manufactured.

[0069] Comparing conventional high-strength bolts with the high-strength bolts prepared in Examples 1 to 5, the high-strength bolts prepared in Examples 1 to 5 are shown in the following table: Example one two three Four five Increased strength 15% 31% 11% 27% 33% Improved moisture resistance 22% 28% 20% 15% 19% It can be seen from the above table that the high-strength bolts used in subways and the processing method thereof proposed by the present invention have obvious improvements, and implementation 2 is the best implementation example.

[0070] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A high-strength bolt used in subways, characterized in that: The raw materials include the following proportions: 1-30 parts of carbon, 1-25 parts of manganese, 1-22 parts of chromium, 1-20 parts of molybdenum, 1-15 parts of nickel, 1-15 parts of silicon, 1-10 parts of titanium, 1-8 parts of sulfur and 1-5 parts of zinc.

2. A high-strength bolt used in subways and a processing method thereof, characterized in that: The following steps are involved: S1: hot melt mixing; S2: cold forging; S3: heat treatment; S4: thread processing; S5: surface treatment; S6: Quality inspection.

3. The high-strength bolt used in subway and the processing method thereof according to claim 2, characterized in that: In the step S1, carbon, manganese, sulfur, chromium, molybdenum, nickel, silicon, titanium and sulfur are placed in a vacuum furnace with a temperature of 600-800 degrees Celsius, preheated for 10-30 minutes, then heated to 1500-2000 degrees Celsius, heated for 10-20 minutes, and finally air-cooled to room temperature to obtain a blank.

4. The high-strength bolt used in subway and the processing method thereof according to claim 2, characterized in that: In the step S2, the blank is placed in a cold heading machine and forged to obtain a bolt blank.

5. The high-strength bolt used in subway and the processing method thereof according to claim 2, characterized in that: In the step S3, the rough bolt blank is heated at 700-850 degrees Celsius for 10-30 minutes, and then heated at 400-500 degrees Celsius for 30-60 minutes.

6. The high-strength bolt used in subway and the processing method thereof according to claim 2, characterized in that: In the step S4, the processed bolt rough blank is turned by a lathe, a thread groove is formed on the bolt rough blank, and then the head of the bolt rough blank is turned to obtain a bolt.

7. The high-strength bolt used in subway and the processing method thereof according to claim 2, characterized in that: In the step S5, the treated high-strength bolt is immersed in molten zinc to form a uniform zinc coating to obtain a high-strength bolt.

8. The high-strength bolt used in subway and the processing method thereof according to claim 2, characterized in that: In the step S6, the size, dimensions and thread groove dimensions of the high-strength bolt are inspected, and finally the high-strength bolt is manufactured.

Citation Information

Patent Citations

  • Titanium aluminum and boron steel and iron material for high strength bolt and preparation method thereof

    CN108070786A

  • High-strength high-temperature-resistant alloy steel and high-strength bolt prepared therefrom

    CN108220791A

  • High-strength wear-resistant bolt and processing technology thereof

    CN110695322A

  • High-strength high-temperature-resistant bolt and preparation process thereof

    CN113215483A

  • Method of manufacturing high strength bolts

    KR1020000042529A