Silicon wafer grinding method
Through multi-stage grinding method and cooling water flushing technology, the problems of increased surface temperature of silicon wafers and difficulty in cleaning by-products in wafer regeneration grinding are solved, and the surface of silicon wafers is smooth, flat and efficient grinding is achieved, improving product yield and reliability sex.
Patent Information
- Application Number
- CN202411346182.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-25
AI Technical Summary
In the existing wafer regeneration grinding process, the surface temperature of the silicon wafer rises rapidly and it is difficult to clean by-products, resulting in a decrease in the grinding rate, changes in morphological uniformity, increasing defects and roughness, and reducing product yield and reliability.
Using a multi-stage grinding method, firstly use high pressure to remove the surface damage layer, then fine grinding is performed under higher pressure, monitoring the grinding pad temperature in real time and cooling down, and finally fine grinding is performed under low pressure, combined with cooling water to rinse and clean the by-products, dynamic Adjust the grinding time to control the temperature.
Effectively reduce surface defects and roughness of silicon wafers, improve morphological uniformity and grinding rate, and improve product yield and reliability.
Smart Images

Figure CN118990316A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of semiconductor technology, and in particular to a silicon wafer grinding method. Background Art
[0002] With the continuous improvement of IC integration, the surface of silicon wafer substrates is required to have better flatness and cleanliness. In actual production, non-graphic silicon wafers are often used to simulate real products and monitor equipment and process conditions. This type of silicon wafer is called a control wafer. After these silicon wafers are used once or multiple times, the surface of the silicon wafer will be damaged and cannot be reused, which is a very large expense in semiconductor production. The wafer reclaim process can reprocess these wafers so that the wafers meet production needs again, thereby reducing costs. After wafer reclaim, the control wafer must control the surface flatness, cleanliness, and the number of particles and defects of a certain size on the surface within the standard range.
[0003] At present, with the development of process and cost considerations, wafer reclaim grinding process also plays an important role in wafer regeneration process. The problems of flattening efficiency, defects and cost faced by this kind of grinding process need to be solved urgently. Due to the large amount of silicon wafer removed, the grinding time is long, the temperature rises quickly during the grinding process, and the by-products in the grinding process are not easy to clean up, resulting in a decrease in grinding rate, changes in the uniformity of silicon wafer surface morphology, and easy defects, which ultimately reduce the yield and reliability of the product.
[0004] Therefore, a silicon wafer grinding method is needed, which can slow down the temperature rise rate during the wafer reclaim grinding process, clean up the by-products generated during the grinding process in time, improve the grinding rate and the uniformity of the silicon wafer surface, reduce the surface defects and roughness of the silicon wafer, and improve the yield and reliability of the product. Summary of the invention
[0005] Therefore, the present invention provides a silicon wafer grinding method to solve the problem that the temperature in the existing wafer regeneration grinding process rises quickly, making it difficult to clean up the by-products in the grinding process, resulting in a decrease in the grinding rate, changes in the uniformity of the silicon wafer surface morphology, and easily causing defects that lead to deterioration of the silicon wafer roughness, ultimately reducing the yield and reliability of the product.
[0006] The present invention provides a silicon wafer grinding method, comprising:
[0007] Providing a silicon wafer, wherein a surface damage layer exists on the surface of the silicon wafer;
[0008] Performing a first grinding process on the silicon wafer under a first pressure using a first grinding disk and a first grinding pad to remove the surface damage layer;
[0009] Performing a second grinding process on the silicon wafer under a second pressure using a second grinding disk and a second grinding pad;
[0010] performing a third grinding process on the silicon wafer under a third pressure using the second grinding disk and the second grinding pad;
[0011] The third pressure is lower than the second pressure.
[0012] Optionally, the second grinding process further includes:
[0013] The temperature of the second polishing pad is monitored in real time. When the temperature of the second polishing pad is greater than a first preset temperature, the second polishing process is stopped and the temperature of the second polishing pad is cooled.
[0014] Optionally, the third grinding process comprises:
[0015] When the temperature of the second polishing pad is lower than a second preset temperature, a third polishing process is performed on the silicon wafer under a third pressure using the second polishing disk and the second polishing pad.
[0016] Optionally, the first pressure is 2psi to 3psi;
[0017] The second pressure is 2 psi to 3 psi;
[0018] The third pressure is 1 psi to 1.5 psi.
[0019] Optionally, the duration of the first grinding process is a first duration T1;
[0020] The duration of the second grinding process is a second duration T2;
[0021] The duration of the third grinding process is a third duration T3;
[0022] The first duration T1 is a fixed time;
[0023] The third time length T3 is determined by the second time length T2, and the third time length T3 is shorter than the second time length T2.
[0024] Optionally, the relationship between the third time length T3 and the second time length T2 is: T3=1 / 3×T2+10s.
[0025] Optionally, the first preset temperature is 35°C to 45°C;
[0026] The second preset temperature is 25°C to 30°C.
[0027] Optionally, the size of the silicon wafer is 12 inches.
[0028] Optionally, after the first grinding process and / or after the third grinding process, the following steps are further included:
[0029] The silicon wafer is cleaned and dried.
[0030] Optionally, the step of cooling the second polishing pad includes:
[0031] The surface of the second polishing pad is rinsed with cooling water to cool the second polishing pad.
[0032] The technical solution of the present invention has the following advantages:
[0033] (1) The silicon wafer grinding method provided by the present invention first uses a first grinding disc and a first grinding pad to perform a first grinding process on the silicon wafer under a first pressure to remove all surface damage layers on the surface of the silicon wafer, and then uses a second grinding disc and a second grinding pad to perform a second grinding process under a higher second pressure to reduce the surface roughness of the silicon wafer and make the surface of the silicon wafer smoother and flatter; finally, uses a second grinding disc and a second grinding pad to perform a third grinding process under a lower third pressure to prevent the temperature of the second grinding pad from rising too fast, improves the morphology of the silicon wafer, increases the process tolerance, and avoids scratches on the surface of the silicon wafer. The silicon wafer grinding method provided by the present invention can reduce surface defects and roughness of the silicon wafer, improve the uniformity of the surface morphology of the silicon wafer and the grinding rate, and thus improve the yield and reliability of the silicon wafer after grinding.
[0034] (2) The silicon wafer grinding method provided by the present invention monitors the temperature of the second grinding pad in real time during the second grinding process. When the temperature of the second grinding pad is greater than the first preset temperature, the second grinding process is stopped and the second grinding pad is cooled. The time of the second grinding process and the temperature of the second grinding pad can be controlled within a certain range to ensure that the time of the second grinding process is not too long and the temperature of the second grinding pad is not too high. The efficiency of the second grinding process can be ensured, the uniformity of the surface morphology and the grinding rate of the silicon wafer are improved, the surface defects and roughness of the silicon wafer are reduced, and the surface of the silicon wafer is made smoother and flatter.
[0035] (3) In the silicon wafer grinding method provided by the present invention, when the temperature of the second grinding pad drops to less than the second preset temperature, the second grinding disc and the second grinding pad are used to perform a third grinding process on the silicon wafer under a third pressure, so that the second grinding pad can be lowered to a lower temperature, and the third grinding process is performed under a lower third pressure, which can prevent the temperature of the second grinding pad from rising too quickly, improve the morphology of the silicon wafer, increase the process tolerance, avoid scratches on the silicon wafer surface, thereby reducing surface defects and roughness of the silicon wafer, and improving the yield and reliability of the silicon wafer after grinding.
[0036] (4) In the silicon wafer grinding method provided by the present invention, the silicon wafer is cleaned and dried after the first grinding process, so that the byproducts and the first grinding liquid generated during the first grinding process can be cleaned in time, and the silicon wafer can be dry-entered and dry-exited on the first grinding disk, thereby reducing the impact on the subsequent second grinding process, reducing the surface defects and roughness of the silicon wafer, and improving the yield and reliability of the product. After the third grinding process, the silicon wafer is cleaned and dried, so that the silicon wafer can be dry-entered and dry-exited on the second grinding disk, which is convenient for observing the product morphology and is conducive to the subsequent process.
[0037] (5) In the silicon wafer grinding method provided by the present invention, the time T3 of the third low-pressure grinding process is dynamically adjusted according to the time T2 of the second high-pressure grinding process, and the third time length T3 is controlled to be less than the second time length T2. This can prevent the temperature of the second grinding pad from rising too quickly, reduce the surface roughness of the silicon wafer, make the surface of the silicon wafer smoother and flatter, and improve the grinding efficiency.
[0038] (6) In the silicon wafer grinding method provided by the present invention, high-pressure cooling water is used to rinse the surface of the second grinding pad to cool it down, which can quickly reduce the temperature of the second grinding pad. At the same time, the by-products and the second grinding liquid generated during the second grinding process can be cleaned up in time, thereby reducing the impact on the subsequent third grinding process, reducing the surface defects and roughness of the silicon wafer, and improving the yield and reliability of the product. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0040] Figure 1 A schematic diagram of a process of a silicon wafer grinding method in the prior art;
[0041] Figure 2 A schematic diagram of a process of a silicon wafer grinding method according to an embodiment of the present invention;
[0042] Figure 3 A schematic diagram of a silicon wafer structure in each step of a silicon wafer grinding method according to an embodiment of the present invention;
[0043] Figure 4 The figure is a schematic diagram of a specific process of a silicon wafer grinding method according to an embodiment of the present invention.
[0044] Description of reference numerals:
[0045] 100-silicon wafer; 200-surface damage layer; 1-first grinding process stop position; 2-second grinding process stop position; 3-third grinding process stop position. DETAILED DESCRIPTION
[0046] In the prior art, such as Figure 1 As shown, a two-step polishing method is often used. First, all damaged layers are removed by the first step of grinding (rough polishing), and then the damage caused by the first step of grinding is repaired by the second step of grinding (fine polishing). The first step of grinding is high-pressure grinding of the first grinding wheel P1 for a fixed time, and the second step of grinding is high-pressure grinding of the second grinding wheel P2 for a fixed time.
[0047] The existing 12-inch silicon wafer chemical mechanical polishing method basically adopts a fixed time in the fine polishing process, and there is no monitoring method for the polishing process. Due to the long polishing time, it is easy to cause the polishing temperature to rise quickly, accelerate the chemical corrosion of the polishing liquid on the silicon wafer surface, and the surface roughness deteriorates. At the same time, the by-products in the polishing process are not easy to clean up, resulting in a decrease in the polishing rate, changes in the surface morphology of the silicon wafer, and easy scratch defects, which ultimately reduce the yield and reliability of the product. In view of the above problems, the present invention mainly improves the problems of surface roughness and defects in the chemical mechanical polishing method in the prior art.
[0048] In order to solve the problem that the temperature in the existing wafer regeneration grinding process rises quickly, making it difficult to clean up the by-products in the grinding process, resulting in a decrease in the grinding rate, a change in the uniformity of the silicon wafer surface morphology, and defects that easily lead to poor roughness of the silicon wafer, ultimately reducing the yield and reliability of the product, the present invention provides a silicon wafer grinding method, comprising: providing a silicon wafer, wherein a surface damage layer exists on the surface of the silicon wafer; performing a first grinding process on the silicon wafer using a first grinding disc and a first grinding pad at a first pressure to remove the surface damage layer; performing a second grinding process on the silicon wafer using a second grinding disc and a second grinding pad at a second pressure; performing a third grinding process on the silicon wafer using the second grinding disc and the second grinding pad at a third pressure; the third pressure is less than the second pressure.
[0049] The technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. In the description of the present invention, it should be noted that the terms "first", "second" and "third" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.
[0050] Example 1
[0051] like Figure 2-Figure 3 As shown, this embodiment provides a silicon wafer grinding method, comprising:
[0052] S101, providing a silicon wafer 100, wherein a surface damage layer 200 exists on the surface of the silicon wafer.
[0053] In a specific implementation, the silicon wafer is a blank silicon wafer or a recycled silicon wafer to be ground, and there is a surface damage layer 200 to be removed on the surface of the silicon wafer 100 .
[0054] S102, using a first grinding disk and a first grinding pad to perform a first grinding process on the silicon wafer 100 under a first pressure to remove the surface damaged layer 200. In some embodiments, the first grinding process also removes part of the surface of the silicon wafer 100.
[0055] In a specific implementation, the silicon wafer 100 is placed on the first grinding disk and the first grinding pad, and the silicon wafer 100 is subjected to a first grinding process under a first pressure to remove all the surface damage layers 200 on the surface of the silicon wafer 100 and part of the surface of the silicon wafer 100, and the silicon wafer 100 is ground to position 1 by the first grinding process. The first grinding process is a coarse grinding process, using a first grinding liquid with larger particles, and the first grinding pad is a hard grinding pad, which can quickly remove a large amount of the surface damage layer 200. The time of the first grinding process is a fixed time.
[0056] S103 , performing a second grinding process on the silicon wafer 100 under a second pressure using a second grinding disk and a second grinding pad.
[0057] In a specific implementation, the silicon wafer 100 is moved onto the second grinding disk and the second grinding pad, and the silicon wafer 100 is subjected to a second grinding process under a second pressure, and the silicon wafer 100 is ground to position 2 through the second grinding process. The second grinding process is fine grinding, and a second grinding liquid with smaller particles is used, and the second grinding pad is a soft grinding pad, which can reduce the surface roughness of the silicon wafer and make the surface of the silicon wafer smooth and flat.
[0058] S104, performing a third grinding process on the silicon wafer 100 at a third pressure using the second grinding disk and the second grinding pad; the third pressure is less than the second pressure.
[0059] In specific implementation, the silicon wafer 100 is still located on the second grinding disk and the second grinding pad, and the third grinding process is performed on the silicon wafer 100 under the third pressure, and the silicon wafer 100 is ground to position 3 by the third grinding process. The second grinding process is fine grinding, using a second grinding liquid with smaller particles, and the second grinding pad is a soft grinding pad, which can reduce the surface roughness of the silicon wafer and make the surface of the silicon wafer smoother and flatter. Among them, the third pressure is less than the second pressure, and the third grinding process can improve the surface morphology of the silicon wafer and improve the process tolerance.
[0060] Those skilled in the art can understand that the first grinding process stop position 1, the second grinding process stop position 2 and the third grinding process stop position 3 are affected by grinding conditions, especially grinding time, and are not fixed positions of the silicon wafer. The positions shown in the figure are only to help illustrate the present solution, and are not intended to limit the present solution.
[0061] The silicon wafer grinding method provided in this embodiment first uses a first grinding disc and a first grinding pad to perform a first grinding process on the silicon wafer 100 under a first pressure to remove all surface damage layers on the silicon wafer surface, and then uses a second grinding disc and a second grinding pad to perform a second grinding process under a higher second pressure to reduce the surface roughness of the silicon wafer and make the surface of the silicon wafer smoother and flatter; finally, the second grinding disc and the second grinding pad are used to perform a third grinding process under a lower third pressure, which can prevent the temperature of the second grinding pad from rising too fast, improve the morphology of the silicon wafer, increase the process tolerance, and avoid scratches on the surface of the silicon wafer. The silicon wafer grinding method provided by the present invention can reduce surface defects and roughness of the silicon wafer, improve the uniformity of the surface morphology of the silicon wafer and the grinding rate, and thus improve the yield and reliability of the silicon wafer after grinding.
[0062] Furthermore, in some embodiments, the second grinding process further includes:
[0063] The temperature of the second polishing pad is monitored in real time. When the temperature of the second polishing pad is greater than a first preset temperature, the second polishing process is stopped and the temperature of the second polishing pad is cooled.
[0064] During specific implementation, during the second grinding process of the silicon wafer 100 using the second grinding disk and the second grinding pad under the second pressure, the temperature of the second grinding pad can be monitored in real time, and the specific monitoring time interval can be set according to actual needs, such as 1s, 2s, etc., which is not limited in this embodiment.
[0065] In order to prevent the second grinding process from being too long, causing the temperature of the second grinding pad to rise too quickly, accelerating the chemical corrosion of the second grinding liquid on the surface of the silicon wafer, and causing the surface roughness to deteriorate, therefore, when the temperature of the second grinding pad is greater than the first preset temperature, the second grinding process is stopped and the second grinding pad is cooled. At this time, the surface of the silicon wafer 100 is basically smooth and flat.
[0066] In the silicon wafer grinding method provided in this embodiment, the temperature of the second grinding pad is monitored in real time during the second grinding process. When the temperature of the second grinding pad is greater than the first preset temperature, the second grinding process is stopped and the second grinding pad is cooled. The time of the second grinding process and the temperature of the second grinding pad can be controlled within a certain range to ensure that the time of the second grinding process is not too long and the temperature of the second grinding pad is not too high. The efficiency of the second grinding process can be guaranteed, the uniformity of the surface morphology and the grinding rate of the silicon wafer are improved, the surface defects and roughness of the silicon wafer are reduced, and the surface of the silicon wafer is made smoother and flatter.
[0067] Furthermore, in some embodiments, the third grinding process comprises:
[0068] When the temperature of the second polishing pad is lower than the second preset temperature, the second polishing disk and the second polishing pad are used to perform a third polishing process on the silicon wafer 100 under a third pressure.
[0069] In specific implementation, too high a grinding pressure may also cause the temperature of the second grinding pad to rise too quickly, accelerating the chemical corrosion of the grinding liquid on the surface of the silicon wafer, resulting in a deterioration of the surface roughness of the silicon wafer. Therefore, when the temperature of the second grinding pad drops to less than the second preset temperature, the second grinding disc and the second grinding pad are used to perform a third grinding process on the silicon wafer 100 under a third pressure, and the third pressure is less than the second pressure.
[0070] The silicon wafer grinding method provided in this embodiment, when the temperature of the second grinding pad drops to less than the second preset temperature, the second grinding disc and the second grinding pad are used to perform a third grinding process on the silicon wafer 100 under a third pressure, so that the second grinding pad can be lowered to a lower temperature, and the third grinding process is performed under a lower third pressure, which can prevent the temperature of the second grinding pad from rising too quickly, improve the silicon wafer morphology, increase the process tolerance, avoid scratches on the silicon wafer surface, thereby reducing surface defects and roughness of the silicon wafer, and improving the yield and reliability of the silicon wafer after grinding.
[0071] Further, in some embodiments, the first pressure is 2psi to 3psi, such as 2psi, 2.4psi, 2.3psi, 3psi;
[0072] The second pressure is 2 psi to 3 psi, such as 2 psi, 2.4 psi, 2.3 psi, 3 psi;
[0073] The third pressure is 1 psi to 1.5 psi, for example, 1 psi, 1.1 psi, 1.3 psi, 1.5 psi.
[0074] Further, in some embodiments, the time of the first grinding process is a first time length T1;
[0075] The duration of the second grinding process is a second duration T2;
[0076] The duration of the third grinding process is a third duration T3;
[0077] The first duration T1 is a fixed time;
[0078] The third time length T3 is determined by the second time length T2, and the third time length T3 is shorter than the second time length T2.
[0079] In specific implementation, the first grinding process is rough grinding, and the second grinding process and the third grinding process are fine grinding. In the rough grinding process, the first grinding time T1 is selected to quickly remove a large amount of surface damage layer. The first grinding time T1 is a fixed time. According to the thickness of the silicon wafer to be ground, the corresponding first grinding time T1 is set. In some examples, the first grinding time T1 is 2 minutes to 3 minutes. In the fine grinding process, the time T2 of the high-pressure second grinding process is determined according to the temperature change of the second grinding pad, and the time T3 of the low-pressure third grinding process is dynamically adjusted according to the high-pressure grinding time T2, and the third grinding time T3 is controlled to be less than the second grinding time T2.
[0080] The silicon wafer grinding method provided in this embodiment dynamically adjusts the time T3 of the third low-pressure grinding process according to the time T2 of the second high-pressure grinding process, and controls the third time length T3 to be less than the second time length T2, so as to prevent the temperature of the second grinding pad from rising too quickly, reduce the surface roughness of the silicon wafer, make the surface of the silicon wafer smoother and flatter, and improve the grinding efficiency.
[0081] Furthermore, in some embodiments, the relationship between the third time length T3 and the second time length T2 is: T3 = 1 / 3 × T2 + 10s.
[0082] By controlling the relationship between the third time length T3 and the second time length T2 as: T3=1 / 3×T2+10s, and the third time length T3 is less than the second time length T2, the time T3 of the low-pressure third grinding process can be dynamically adjusted according to the time T2 of the high-pressure second grinding process to prevent the temperature of the second grinding pad from rising too quickly, thereby reducing the surface roughness of the silicon wafer, making the surface of the silicon wafer smoother and flatter, and improving the grinding efficiency.
[0083] Furthermore, in some embodiments, the relationship between the third duration T3 and the second duration T2 is: T3 = 1 / 3 × T2.
[0084] Further, in some embodiments, the first preset temperature is 35°C to 45°C, for example, 35°C, 38°C, 40°C, 45°C;
[0085] The second preset temperature is 25°C to 30°C, for example, 25°C, 26°C, 28°C, 30°C;
[0086] Furthermore, in some embodiments, the size of the silicon wafer 100 is 12 inches.
[0087] The existing chemical mechanical polishing method for 12-inch silicon wafers basically adopts a fixed time in the fine polishing process, and there is no monitoring method for the polishing process. Due to the long polishing time, the polishing temperature is likely to rise quickly, which accelerates the chemical corrosion of the polishing liquid on the silicon wafer surface and worsens the surface roughness. At the same time, the by-products in the grinding process are not easy to clean up, resulting in a decrease in the grinding rate, changes in the surface morphology of the silicon wafer, and easy scratch defects, which ultimately reduce the yield and reliability of the product.
[0088] The 12-inch silicon wafer grinding method provided in this embodiment has fine grinding divided into a high-pressure second grinding process and a low-pressure third grinding process. Compared with the fixed-time fine polishing process in the existing 12-inch silicon wafer chemical mechanical grinding method, this method can avoid too high grinding temperature during high-pressure fine polishing by controlling the temperature of the second grinding pad; and slow down the temperature rise rate during low-pressure fine polishing, clean up the by-products generated during the grinding process in time, improve the grinding rate and uniformity of the silicon wafer surface, reduce silicon wafer surface defects and roughness, and improve the yield and reliability of the product.
[0089] Further, in some embodiments, after the first grinding process and / or after the third grinding process, the following steps are further included:
[0090] The silicon wafer 100 is cleaned and dried.
[0091] The silicon wafer grinding method provided in this embodiment performs cleaning and drying of the silicon wafer after the first grinding process, and can timely clean the byproducts and the first grinding liquid generated during the first grinding process, so as to achieve dry entry and exit of the silicon wafer on the first grinding disk, reduce the impact on the subsequent second grinding process, reduce the surface defects and roughness of the silicon wafer, and improve the yield and reliability of the product. After the third grinding process, the silicon wafer is cleaned and dried, so as to achieve dry entry and exit of the silicon wafer on the second grinding disk, which is convenient for observing the product morphology and is conducive to the subsequent processes.
[0092] Furthermore, in some embodiments, the step of cooling the second polishing pad includes:
[0093] The surface of the second polishing pad is rinsed with cooling water to cool the second polishing pad.
[0094] During specific implementation, high-pressure cooling water is used to rinse the surface of the second polishing pad to cool it down, which can quickly reduce the temperature of the second polishing pad. At the same time, the by-products and the second polishing liquid generated during the second polishing process can be cleaned up in time, thereby reducing the impact on the subsequent third polishing process, reducing surface defects and roughness of silicon wafers, and improving product yield and reliability.
[0095] refer to Figure 3-4 The following provides a specific process of a silicon wafer grinding method, including steps S201-S207:
[0096] S201, providing a silicon wafer 100, wherein a surface damage layer 200 exists on the surface of the silicon wafer 100, and the size of the silicon wafer 100 is 12 inches.
[0097] S202 , performing a first grinding process on the silicon wafer 100 under a first pressure using a first grinding disk and a first grinding pad to remove the surface damaged layer 200 .
[0098] The first pressure is 2 psi to 3 psi, and the time of the first grinding process is a first time length T1. The first time length T1 is a fixed time.
[0099] In a specific implementation, the silicon wafer 100 is placed on the first grinding disk and the first grinding pad, and the silicon wafer 100 is subjected to a first grinding process under a first pressure to remove all the surface damage layers 200 on the surface of the silicon wafer 100 and part of the surface of the silicon wafer 100, and the silicon wafer 100 is ground to position 1 through the first grinding process. The first grinding process is coarse grinding, using a first grinding liquid with larger particles, and the first grinding pad is a hard grinding pad, which can quickly remove a large amount of the surface damage layer 200.
[0100] S203, cleaning and drying the silicon wafer 100.
[0101] The silicon wafer 100 is cleaned and dried after the first grinding process, so as to timely clean the byproducts and the first grinding liquid generated during the first grinding process, realize dry entry and exit of the silicon wafer on the first grinding disk, reduce the impact on the subsequent second grinding process, reduce the surface defects and roughness of the silicon wafer 100, and improve the yield and reliability of the product.
[0102] S204, performing a second grinding process on the silicon wafer 100 at a second pressure using a second grinding disk and a second grinding pad. The second pressure is 2 psi to 3 psi.
[0103] In specific implementation, the silicon wafer 100 is moved onto the second grinding disk and the second grinding pad, and the second grinding process is performed on the silicon wafer 100 under the second pressure. The second grinding process is fine grinding, using a second grinding liquid with smaller particles, and the second grinding pad is a soft grinding pad, which can reduce the surface roughness of the silicon wafer 100 and make the surface of the silicon wafer 100 smooth and flat.
[0104] S205, monitoring the temperature of the second polishing pad in real time, when the temperature of the second polishing pad is greater than the first preset temperature, stopping the second polishing process, and flushing the surface of the second polishing pad with cooling water to cool the second polishing pad.
[0105] The first preset temperature is 35° C. to 45° C., the time of the second grinding process is a second time length T2, and the second time length T2 is determined by the temperature change of the second grinding pad.
[0106] In specific implementation, during the second grinding process of the silicon wafer 100 using the second grinding disc and the second grinding pad under the second pressure, the temperature of the second grinding pad is monitored in real time, and the specific monitoring time interval can be set according to actual needs, such as 1s, 2s, etc., which is not limited in this embodiment. In order to prevent the second grinding process from taking too long, causing the temperature of the second grinding pad to rise too quickly, accelerating the chemical corrosion of the second grinding liquid on the surface of the silicon wafer 100, and causing the surface roughness to deteriorate, therefore, when the temperature of the second grinding pad is greater than the first preset temperature, the second grinding process is stopped, at which time the surface of the silicon wafer 100 is basically smooth and flat, and the silicon wafer 100 is ground to position 2.
[0107] The second time length T2 is determined by the temperature change of the second polishing pad, which can ensure that the time of the second polishing process is not too long and the temperature of the second polishing pad is not too high, thereby improving the efficiency of the second polishing process, improving the surface morphology uniformity and polishing rate of the silicon wafer, reducing the surface defects and roughness of the silicon wafer, and making the surface of the silicon wafer smooth and flat.
[0108] High-pressure cooling water is then used to rinse the surface of the second polishing pad to cool it down, which can quickly reduce the temperature of the second polishing pad. At the same time, the by-products and the second polishing liquid generated during the second polishing process can be cleaned up in time, reducing the impact on the subsequent third polishing process, reducing surface defects and roughness of silicon wafers, and improving product yield and reliability.
[0109] S206, when the temperature of the second polishing pad is lower than a second preset temperature, performing a third polishing process on the silicon wafer at a third pressure using the second polishing disk and the second polishing pad, wherein the third pressure is lower than the second pressure.
[0110] The second preset temperature is 25°C to 30°C, the time of the third grinding process is a third time length T3; the third time length T3 is determined by the second time length T2, and the third time length T3 is less than the second time length T2. And the relationship between the third time length T3 and the second time length T2 is: T3 = 1 / 3 × T2 + 10s.
[0111] In specific implementation, the silicon wafer 100 is still located on the second grinding disk and the second grinding pad, and the third grinding process is performed on the silicon wafer 100 under the third pressure, and the silicon wafer 100 is ground to position 3 by the third grinding process. The second grinding process is fine grinding, using a second grinding liquid with smaller particles, and the second grinding pad is a soft grinding pad, which can reduce the surface roughness of the silicon wafer and make the surface of the silicon wafer smoother and flatter. Among them, the third pressure is less than the second pressure, and the third grinding process can improve the surface morphology of the silicon wafer and improve the process tolerance.
[0112] The time T3 of the third low-pressure grinding process is dynamically adjusted according to the time T2 of the second high-pressure grinding process. At the same time, by controlling the third time length T3 to be less than the second time length T2, the temperature of the second grinding pad can be prevented from rising too quickly, the surface roughness of the silicon wafer 100 can be reduced, the surface of the silicon wafer 100 can be made smoother and flatter, and the grinding efficiency can be improved.
[0113] S207, cleaning and drying the silicon wafer 100.
[0114] After the third grinding process, the silicon wafer 100 is cleaned and dried, so that the silicon wafer 100 can be dry-entered and dry-exited from the second grinding disk, which is convenient for observing the product morphology and is beneficial to the subsequent processes.
[0115] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A silicon wafer grinding method, characterized in that: include: Providing a silicon wafer, wherein a surface damage layer exists on the surface of the silicon wafer; Performing a first grinding process on the silicon wafer under a first pressure using a first grinding disk and a first grinding pad to remove the surface damage layer; Performing a second grinding process on the silicon wafer under a second pressure using a second grinding disk and a second grinding pad; performing a third grinding process on the silicon wafer under a third pressure using the second grinding disk and the second grinding pad; The third pressure is lower than the second pressure.
2. The silicon wafer grinding method according to claim 1, characterized in that: The second grinding process also includes: The temperature of the second polishing pad is monitored in real time. When the temperature of the second polishing pad is greater than a first preset temperature, the second polishing process is stopped and the temperature of the second polishing pad is cooled.
3. The silicon wafer grinding method according to claim 2, characterized in that: The steps of the third grinding process include: When the temperature of the second polishing pad is lower than a second preset temperature, a third polishing process is performed on the silicon wafer under a third pressure using the second polishing disk and the second polishing pad.
4. The silicon wafer grinding method according to claim 3, characterized in that: The first pressure is 2 psi to 3 psi; The second pressure is 2 psi to 3 psi; The third pressure is 1 psi to 1.5 psi.
5. The silicon wafer grinding method according to claim 3, characterized in that: The duration of the first grinding process is a first duration T1; The duration of the second grinding process is a second duration T2; The duration of the third grinding process is a third duration T3; The first duration T1 is a fixed time; The third duration T3 is determined by the second duration T2, and the third duration T3 is shorter than the second duration T2.
6. The silicon wafer grinding method according to claim 5, characterized in that: The relationship between the third time length T3 and the second time length T2 is: T3=1 / 3×T2+10s.
7. The silicon wafer grinding method according to claim 3, characterized in that: The first preset temperature is 35°C to 45°C; The second preset temperature is 25°C to 30°C.
8. The silicon wafer grinding method according to claim 1, characterized in that: The size of the silicon wafer is 12 inches.
9. The silicon wafer grinding method according to claim 1, characterized in that: After the first grinding process and / or after the third grinding process, the following further comprises: The silicon wafer is cleaned and dried.
10. The silicon wafer grinding method according to claim 2, characterized in that: The step of cooling the second polishing pad comprises: The surface of the second polishing pad is rinsed with cooling water to cool the second polishing pad.
Citation Information
Patent Citations
Chemical mechanical grinding method for interlayer dielectric layer
CN101961852A
Surface grinding method for silicon carbide wafer
CN114800252A
Surface treatment method of semiconductor structure
CN117067103A
Wafer grinding method, device and equipment
CN117773767A
Chemical mechanical polishing method
CN117798811A