Biaxially oriented polyester film with flame-retardant function and preparation method of biaxially oriented polyester film

By using thermally stable and PET-compatible flame retardant in BOPET films, a bidirectional tensile polyester film with excellent flame retardant, mechanical and optical properties is prepared, which solves the high-temperature processing process of flame retardant in the prior art. Loss and performance degradation issues.

CN118991195APending Publication Date: 2024-11-22康辉南通新材料科技有限公司

Patent Information

Application Number
CN202410893079.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing BOPET films are flammable. Flame retardant may affect transparency and mechanical properties while improving flame retardant properties, and decompose during high-temperature processing to lead to loss of flame retardant properties.

Method used

Polyethylene terephthalate and flame retardant (such as ammonium polyphosphate, magnesium aluminum bihydroxide) are used as the core layer raw materials, and bidirectional stretching is used to prepare a bidirectional pulling with flame retardant function by extruding the casting sheet and bidirectional stretching treatment. Extend polyester film to ensure thermal stability of the flame retardant and good compatibility with PET.

Benefits of technology

While improving the flame retardant performance, the transparency and mechanical properties of the film are maintained, ensuring that the flame retardant performance does not fail during high-temperature processing, and significantly improving the flame retardant, mechanical and optical properties of BOPET films.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a biaxially oriented polyester film with a flame-retardant function and a preparation method of the biaxially oriented polyester film. The biaxially oriented polyester film comprises a core layer, an upper surface layer and a lower surface layer, wherein the upper surface layer and the lower surface layer are arranged on the upper surface and the lower surface of the core layer respectively; the preparation raw materials of the core layer comprise a flame-retardant master batch and a PET (Polyethylene Terephthalate) slice; the preparation raw materials of the upper surface layer and the lower surface layer comprise anti-sticking master batches; wherein the flame-retardant master batch comprises polyethylene glycol terephthalate and a flame retardant, and the flame retardant is selected from at least one of ammonium polyphosphate, aluminum diethyl hypophosphite and magnesium-aluminum double hydroxide. The flame retardant adopted by the invention has better thermal stability, and cannot be decomposed in the high-temperature processing process of the film, so that the stability of the flame retardant property is ensured. The flame retardant used in the invention has organic groups, has good compatibility with PET, and does not reduce the mechanical properties and transparency of the biaxially oriented polyester film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiments of the present invention relate to the technical field of polymer material preparation, and in particular to a biaxially oriented polyester film with flame retardant function. Background Art

[0002] BOPET (biaxially oriented polyester) film is a polymer material widely used in packaging, electronics, optics and other fields. However, BOPET film itself is flammable, which limits its application to a certain extent. Therefore, how to improve the flame retardant properties of BOPET film is one of the current research hotspots.

[0003] At present, the existing solution is mainly to add flame retardants during the preparation of polyester film to improve its flame retardant properties. For example, halogen flame retardants, phosphorus flame retardants, etc. can be added. However, while these flame retardants improve the flame retardant properties, they may affect the transparency and mechanical properties of the film, or may decompose during high-temperature processing, resulting in a loss of flame retardant properties. Summary of the invention

[0004] 1. Technical issues to be resolved

[0005] The technical problem to be solved by the present invention is to solve the technical problem of how to improve the flame retardant properties of the film while ensuring that the flame retardant properties of the film are not lost during high-temperature processing, and at the same time ensuring that the prepared film has good mechanical properties and transparency.

[0006] (II) Technical solution

[0007] In order to solve the above technical problems, the present invention provides, on the one hand, a biaxially oriented polyester film with flame retardant function, comprising a core layer, an upper surface layer and a lower surface layer respectively arranged on the upper surface and the lower surface of the core layer; the raw materials for preparing the core layer include a flame retardant masterbatch and PET slices; the raw materials for preparing the upper surface layer and the lower surface layer include an anti-sticking masterbatch; wherein the flame retardant masterbatch includes polyethylene terephthalate and a flame retardant, and the flame retardant is selected from at least one of ammonium polyphosphate, diethyl aluminum hypophosphite and magnesium aluminum double hydroxide.

[0008] In one embodiment, the flame retardant is ammonium polyphosphate, diethyl aluminum hypophosphite or magnesium aluminum double hydroxide; or, the flame retardant is selected from any two of ammonium polyphosphate, diethyl aluminum hypophosphite and magnesium aluminum double hydroxide; or, the flame retardant is a mixture of ammonium polyphosphate, diethyl aluminum hypophosphite and magnesium aluminum double hydroxide, preferably mixed in a mass ratio of 1:1:1.

[0009] In one embodiment, the mass percentage content of the flame retardant in the flame retardant masterbatch is 10-50%. Preferably, the mass percentage content of the flame retardant in the flame retardant masterbatch is 20-50%.

[0010] In one embodiment, the raw materials for preparing the flame retardant masterbatch are polyethylene terephthalate and diethyl aluminum hypophosphite; or, the raw materials for preparing the flame retardant masterbatch are polyethylene terephthalate and diethyl aluminum hypophosphite, ammonium polyphosphate, and magnesium aluminum double hydroxide.

[0011] In one embodiment, the mass ratio of the flame retardant masterbatch and the PET chips in the raw materials for preparing the core layer is (60-90): (10-40).

[0012] In one embodiment, the raw materials for preparing the anti-sticking masterbatch include polyethylene terephthalate and an opening agent, and the mass ratio of the opening agent to polyethylene terephthalate is (4-6):(94-96), preferably 5:95; preferably, the opening agent is SiO2.

[0013] In one embodiment, the ratio of the mass of the core layer to the total mass of the upper surface layer and the lower surface layer is (50-90): (10-50).

[0014] In one embodiment, the upper surface layer and the lower surface layer are prepared from the same raw materials, and the upper surface layer and the lower surface layer have the same thickness.

[0015] On the one hand, the present invention also provides a method for preparing a biaxially oriented polyester film with flame retardant function as described in any of the above items, comprising: melt blending polyethylene terephthalate and a flame retardant to obtain a flame retardant masterbatch containing the flame retardant; melt blending polyethylene terephthalate and an opening agent to obtain an anti-sticking masterbatch containing the opening agent; mixing the flame retardant masterbatch with PET slices as the core layer raw material of the film, and using the anti-sticking masterbatch as the raw material for the upper surface layer and the lower surface layer of the film; subjecting the core layer raw material, the upper surface layer raw material and the lower surface layer raw material to extrusion casting, biaxial stretching and heat setting treatment to prepare a biaxially oriented polyester film.

[0016] In one embodiment, the process parameters during melt blending are: extrusion temperature of 260-280°C, screw speed of 80-120rpm; and / or, the process parameters during biaxial stretching are: stretching temperature of 70-100°C for longitudinal stretching, stretching ratio of 3-3.5 times, stretching temperature of 100-120°C for transverse stretching, stretching ratio of 3-4 times; and / or, the process parameters of heat setting treatment are: heat setting temperature of 190-230°C, time of 10-20s.

[0017] (III) Beneficial effects

[0018] The above technical solution of the present invention has the following advantages:

[0019] The flame retardant used in the present invention has good thermal stability and will not decompose during high-temperature processing of the film, thereby ensuring the stability of the flame retardant performance.

[0020] The flame retardant used in the present invention has an organic group, has good compatibility with PET, and will not reduce the mechanical properties and transparency of the biaxially stretched polyester film. DETAILED DESCRIPTION

[0021] In order to more clearly understand the above-mentioned objectives, features and advantages of the present invention, the scheme of the present invention will be further described below. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

[0022] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein; it is obvious that the embodiments in the specification are only part of the embodiments of the present invention, rather than all of the embodiments.

[0023] In the present invention, unless otherwise specified, the raw materials and equipment used can be purchased from the market or are commonly used in the art. The methods in the embodiments, unless otherwise specified, are all conventional methods in the art.

[0024] The present invention will be further described in detail below with reference to the embodiments.

[0025] Embodiment 1

[0026] The preparation raw materials include: polyethylene terephthalate (PET slices), diethyl aluminum hypophosphite (ADP), and SiO2.

[0027] The preparation steps include:

[0028] Step 1: Prepare raw materials. First, prepare pure polyethylene terephthalate (PET) chips as the base material, with an intrinsic viscosity of 0.68 dL / g and a melting point of 250°C. At the same time, prepare the flame retardant diethyl aluminum hypophosphite (ADP) with a purity of 98%.

[0029] Step 2: Prepare flame retardant masterbatch. Mix the flame retardant ADP and PET chips evenly according to the mass ratio. The flame retardant and chips are melt blended in a twin-screw extruder, the extrusion temperature is set to 260°C, the screw speed is 80rpm, and after extrusion granulation, a flame retardant masterbatch containing flame retardant additives is obtained. The anti-sticking masterbatch is obtained by melt blending, extruding and granulating SiO2 and PET chips, wherein the mass ratio of SiO2 to PET is 5:95, the extrusion temperature is set to 260°C, and the screw speed is 80rpm.

[0030] Step 3: Prepare BOPET film. The flame retardant masterbatch obtained in step 2 is mixed evenly with the PET slices according to the mass ratio to serve as the core layer of the ABA structure of the PET film. The upper and lower surface layers are prepared with the same raw materials and thickness, and the raw materials for the upper and lower surface layers are anti-sticking masterbatch. The raw material melt is first extruded into a sheet, and then subjected to biaxial stretching and heat setting treatment to finally obtain a flame retardant and transparent BOPET film. The stretching temperature for longitudinal stretching is 70°C, and the stretching ratio is 3 times. The stretching temperature for transverse stretching is 100°C, and the stretching ratio is 3 times. The heat setting temperature is 190°C, and the time is 20s.

[0031] Step 4: Post-treatment. The BOPET film obtained in step 3 is cooled, rolled and slit to obtain a flame-retardant polyester film with a thickness of 50 μm. During the entire preparation process, it is necessary to keep the environment clean to avoid the influence of impurities on the film properties. At the same time, it is also necessary to control the operating parameters of each step to ensure the stability of the film quality. The sample formula is shown in Table 1.

[0032] Table 1 Formulations of different samples

[0033]

[0034]

[0035] The above samples were tested. Among them, LOI: tested according to GB / T 2406-2009 standard; UL-94: tested according to GB / T 2408-2021 standard; tensile strength and elongation at break: tested according to ASTMD-882 standard. Light transmittance: tested according to ASTMD-1746 standard. Haze: tested according to ASTMD-1003 standard.

[0036] Table 2 below shows the limiting oxygen index LOI, vertical burning grade UL-94, tensile strength at break, elongation at break, light transmittance and haze of sample 1, sample 2, sample 3 and sample 4. It can be seen that the BOPET composite material prepared by the present invention has excellent flame retardant properties, mechanical properties and optical properties.

[0037] Table 2 Performance test data of BOPET composite materials

[0038]

[0039] Embodiment 2

[0040] The preparation raw materials include: polyethylene terephthalate (PET slices), diethyl aluminum hypophosphite (ADP), and SiO2.

[0041] The preparation steps include:

[0042] Step 1: Prepare raw materials. First, prepare pure polyethylene terephthalate (PET) chips as the base material, with an intrinsic viscosity of 0.68 dL / g and a melting point of 250°C. At the same time, prepare the flame retardant diethyl aluminum hypophosphite (ADP) with a purity of 98%.

[0043] Step 2: Prepare flame retardant masterbatch. Mix the flame retardant ADP and PET chips evenly according to the mass ratio. The flame retardant and chips are melt blended in a twin-screw extruder, the extrusion temperature is set to 270°C, the screw speed is 100rpm, and after extrusion granulation, a flame retardant masterbatch containing flame retardant additives is obtained. The anti-sticking masterbatch is obtained by melt blending, extruding and granulating SiO2 and PET chips, wherein the mass ratio of SiO2 to PET is 5:95, the extrusion temperature is set to 270°C, and the screw speed is 100rpm.

[0044] Step 3: Prepare BOPET film. The flame retardant masterbatch obtained in step 2 is mixed evenly with the PET slices according to the mass ratio to serve as the core layer of the ABA structure of the PET film. The upper and lower surface layers are prepared with the same raw materials and thickness, and the raw materials for the upper and lower surface layers are anti-sticking masterbatch. The raw material melt is first extruded into a sheet, then biaxially stretched and heat-set to finally obtain a flame-retardant and transparent BOPET film. The stretching temperature for longitudinal stretching is 85°C, and the stretching ratio is 3.2 times. The stretching temperature for transverse stretching is 110°C, and the stretching ratio is 3.5 times. The heat setting temperature is 210°C, and the time is 15s.

[0045] Step 4: Post-treatment. The BOPET film obtained in step 3 is cooled, rolled and slit to obtain a flame-retardant polyester film with a thickness of 50 μm. During the entire preparation process, it is necessary to keep the environment clean to avoid the influence of impurities on the film properties. At the same time, it is also necessary to control the operating parameters of each step to ensure the stability of the film quality. The sample formula is shown in Table 3.

[0046] Table 3 Formulations of different samples

[0047]

[0048]

[0049] The above samples were tested. Among them, LOI: tested according to GB / T 2406-2009 standard; UL-94: tested according to GB / T 2408-2021 standard; tensile strength and elongation at break: tested according to ASTMD-882 standard. Light transmittance: tested according to ASTMD-1746 standard. Haze: tested according to ASTMD-1003 standard.

[0050] Table 4 below shows the limiting oxygen index LOI, vertical burning grade UL-94, tensile strength at break, elongation at break, light transmittance and haze of sample 1, sample 2, sample 3 and sample 4. It can be seen that the BOPET composite material prepared by the present invention has excellent flame retardant properties, mechanical properties and optical properties.

[0051] Table 4 Performance test data of BOPET composite materials

[0052]

[0053]

[0054] Embodiment 3

[0055] The preparation raw materials include: polyethylene terephthalate (PET slices), ammonium polyphosphate (APP), diethylaluminum hypophosphite (ADP), magnesium aluminum double hydroxide (LDH), and SiO2.

[0056] The preparation steps include:

[0057] Step 1: Prepare the raw materials. First, you need to prepare pure polyethylene terephthalate (PET) chips as the base material, with an intrinsic viscosity of 0.68dL / g and a melting point of 250°C. At the same time, you need to prepare a compounded flame retardant, which is a mixture of ammonium polyphosphate (APP), diethyl aluminum hypophosphite (ADP) and magnesium aluminum double hydroxide (LDH). The mass ratio of the three is 1:1:1, and the purity of the flame retardant is 98%.

[0058] Step 2: Prepare flame retardant masterbatch. Mix the flame retardant and PET chips evenly according to the mass ratio. The flame retardant and chips are melt blended in a twin-screw extruder, the extrusion temperature is set to 280°C, the screw speed is 120rpm, and after extrusion granulation, a flame retardant masterbatch containing flame retardant additives is obtained. The anti-sticking masterbatch is obtained by melt blending, extruding and granulating SiO2 and PET chips, wherein the mass ratio of SiO2 to PET is 5:95, the extrusion temperature is set to 280°C, and the screw speed is 120rpm.

[0059] Step 3: Prepare BOPET film. The flame retardant masterbatch obtained in step 2 is mixed evenly with the PET slices according to the mass ratio to serve as the core layer of the ABA structure of the PET film. The upper and lower surface layers are prepared with the same raw materials and thickness, and the raw materials for the upper and lower surface layers are anti-sticking masterbatch. The raw material melt is first extruded into a sheet, then biaxially stretched and heat-set to finally obtain a flame-retardant and transparent BOPET film. The stretching temperature for longitudinal stretching is 100°C, and the stretching ratio is 3.5 times. The stretching temperature for transverse stretching is 120°C, and the stretching ratio is 4 times. The heat setting temperature is 230°C, and the time is 10s.

[0060] Step 4: Post-treatment. The BOPET film obtained in step 3 is cooled, rolled and slit to obtain a flame-retardant polyester film with a thickness of 50 μm. During the entire preparation process, it is necessary to keep the environment clean to avoid the influence of impurities on the film properties. At the same time, it is also necessary to control the operating parameters of each step to ensure the stability of the film quality. The sample formula is shown in Table 5.

[0061] Table 5 Formulations of different samples

[0062]

[0063] The above samples were tested. Among them, LOI: tested according to GB / T 2406-2009 standard; UL-94: tested according to GB / T 2408-2021 standard; tensile strength and elongation at break: tested according to ASTMD-882 standard. Light transmittance: tested according to ASTMD-1746 standard. Haze: tested according to ASTMD-1003 standard.

[0064] Table 6 shows the limiting oxygen index LOI, vertical burning grade UL-94, tensile strength at break, elongation at break, light transmittance and haze of sample 1, sample 2, sample 3 and sample 4. It can be seen that the compound flame retardant has a better flame retardant effect on BOPET, and the prepared BOPET composite material has excellent flame retardant properties, mechanical properties and optical properties.

[0065] Table 6 Performance test data of BOPET composite materials

[0066]

[0067]

[0068] The flame retardant used in the present invention has good thermal stability and will not decompose during the high-temperature processing of BOPET, thereby ensuring the stability of the flame retardant performance and solving the problem of flame retardant decomposition during high-temperature processing in the prior art leading to loss of flame retardant performance.

[0069] The flame retardant in this embodiment has an organic group and has good compatibility with PET. Even if a large amount is added, it will not significantly reduce the mechanical properties of the polyester film. This solves the problem in the prior art that the flame retardant has poor compatibility with PET and may significantly reduce the mechanical properties of the polyester film when added in a large amount.

[0070] After adding the flame retardant in this embodiment, the BOPET film maintains good transparency while improving the flame retardant performance, solving the problem that the flame retardant may affect the transparency of the film in the prior art. In general, the BOPET film of the present invention has significantly improved flame retardant performance, mechanical properties and transparency, and has high practical value and broad application prospects.

[0071] In addition, it should be noted that, in this embodiment, silane coupling agent (KH550, KH560) can be used to modify the surface of the flame retardant to increase its compatibility with PET, thereby improving the flame retardant effect of the flame retardant while ensuring the mechanical properties of PET. That is, in this embodiment, the above flame retardant can be surface modified before compounding.

[0072] It should be clear that the present invention is not limited to the specific steps and structures described above. In addition, for the sake of brevity, detailed descriptions of known methods and technologies are omitted here.

[0073] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A biaxially oriented polyester film with flame retardant function, Features: It includes a core layer, an upper surface layer and a lower surface layer respectively arranged on the upper surface and the lower surface of the core layer; The raw materials for preparing the core layer include flame retardant masterbatch and PET slices; the raw materials for preparing the upper surface layer and the lower surface layer include anti-sticking masterbatch; The flame retardant masterbatch comprises polyethylene terephthalate and a flame retardant, and the flame retardant is selected from at least one of ammonium polyphosphate, diethyl aluminum hypophosphite and magnesium aluminum double hydroxide.

2. The biaxially oriented polyester film with flame retardant function according to claim 1, Features: The flame retardant is ammonium polyphosphate, diethyl aluminum hypophosphite or magnesium aluminum double hydroxide; or, the flame retardant is selected from any two of ammonium polyphosphate, diethyl aluminum hypophosphite and magnesium aluminum double hydroxide; or, the flame retardant is a mixture of ammonium polyphosphate, diethyl aluminum hypophosphite and magnesium aluminum double hydroxide, preferably mixed in a mass ratio of 1:1:

1.

3. The biaxially oriented polyester film with flame retardant function according to claim 1 or 2, Features: The mass percentage content of the flame retardant in the flame retardant masterbatch is 10-50%, preferably, the mass percentage content of the flame retardant in the flame retardant masterbatch is 20-50%.

4. The biaxially oriented polyester film with flame retardant function according to claim 2 or 3, Features: The raw materials for preparing the flame retardant masterbatch are polyethylene terephthalate and diethyl aluminum hypophosphite; or, the raw materials for preparing the flame retardant masterbatch are polyethylene terephthalate and diethyl aluminum hypophosphite, ammonium polyphosphate, and magnesium aluminum double hydroxide.

5. The biaxially oriented polyester film with flame retardant function according to any one of claims 1 to 4, Features: The mass ratio of the flame retardant masterbatch and the PET chips in the raw materials for preparing the core layer is (60-90): (10-40).

6. The biaxially oriented polyester film with flame retardant function according to any one of claims 1 to 5, Features: The raw materials for preparing the anti-sticking masterbatch include polyethylene terephthalate and an opening agent, and the mass ratio of the opening agent to the polyethylene terephthalate is (4-6): (94-96), preferably 5:95; preferably, the opening agent is SiO 2 .

7. The biaxially oriented polyester film with flame retardant function according to any one of claims 1 to 6, Features: The ratio of the mass of the core layer to the total mass of the upper surface layer and the lower surface layer is (50-90): (10-50).

8. The biaxially oriented polyester film with flame retardant function according to claim 7, Features: The upper surface layer and the lower surface layer are prepared from the same raw materials, and have the same thickness.

9. A method for preparing the biaxially oriented polyester film with flame retardant function according to any one of claims 1 to 8, Features: The polyethylene terephthalate and the flame retardant are melt-blended to obtain a flame retardant masterbatch containing the flame retardant; The polyethylene terephthalate and the opening agent are melt-blended to obtain an anti-sticking masterbatch containing the opening agent; The flame retardant masterbatch is mixed with PET chips to be used as the core layer material of the film, and the anti-sticking masterbatch is used as the material for the upper and lower surface layers of the film; The raw materials of the core layer, the upper surface layer and the lower surface layer are subjected to extrusion casting, biaxial stretching and heat setting treatment to prepare a biaxially stretched polyester film.

10. The preparation method according to claim 9, Features: The process parameters during melt blending are: extrusion temperature of 260-280°C, screw speed of 80-120rpm; and / or, The process parameters during biaxial stretching are: the stretching temperature of longitudinal stretching is 70-100°C, the stretching ratio is 3-3.5 times, the stretching temperature of transverse stretching is 100-120°C, the stretching ratio is 3-4 times; and / or, The process parameters of the heat setting treatment are: heat setting temperature is 190-230°C, and the time is 10-20s.

Citation Information

Patent Citations

  • Migration resistant and high flame retardant halogen-free flame retardant system used for thermoplastic elastomers

    CN103694499A

  • Chemical medium-resistant halogen-free flame-retardant insulating composite material and preparation method thereof

    CN108943950A

  • Flame-retardant black dual-direction stretching polyester thin film and preparation method thereof

    CN109130232A

  • Biaxial stretching polyester film ultra-low in shrinkage rate and high in flame retardance and preparation method thereof

    CN110116533A

  • Antibacterial biaxially oriented polyester film and preparation method thereof

    CN111331989A

Cited By

  • Thin-film flame-retardant PET (polyethylene terephthalate) material and preparation method thereof