Lightning-protection heat-storage anti-icing protective film suitable for front edge of wind power blade and preparation method of lightning-protection heat-storage anti-icing protective film

By applying flexible silicone aerogel thermal insulation fiber and hydrated salt/SiC composite phase change filler heat storage protection film on wind power blades, the problem of icing and lightning strikes in extreme weather is solved, and the power generation efficiency and safety are improved reduces operation and maintenance costs.

CN118991203AActive Publication Date: 2024-11-22HUANENG NEW ENERGY (MENGXI) CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411101438.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

Wind power blades are prone to freezing and are difficult to prevent lightning in extreme weather conditions, which affects power generation efficiency and safety.

Method used

The heat-insulating fiber and heat-storage protection film are provided on the blade substrate. The heat-insulating fiber is a flexible silicone aerogel composite fiber. The heat-storage protection film is made of hydrated salt/SiC composite phase change filler and aqueous polyaspartic acid ester. The resin is composed of cross-linked by bonding coatings and contains modified nanoboronitride to improve insulation properties.

Benefits of technology

Effectively prevent the blades from freezing, improve the power generation efficiency and safety of wind turbines, reduce operation and maintenance costs, and at the same time, do not increase the weight of the blades, and enhance insulation and thermal conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118991203A_ABST
    Figure CN118991203A_ABST
Patent Text Reader

Abstract

The invention discloses an anti-thunder heat-storage anti-icing protective film suitable for the front edge of a wind power blade and a preparation method of the anti-thunder heat-storage anti-icing protective film, and belongs to the technical field of wind power blades. According to the high-conductivity heat storage anti-icing film, heat insulation fibers and a heat storage protection film are arranged on a blade base material from inside to outside, the heat insulation fibers are flexible organic silicon aerogel composite fibers, and the heat storage protection film is formed by crosslinking hydrated salt / SiC composite phase change filler and water-based polyaspartic acid ester resin through a bonding coating; the heat storage protection film is arranged on the outermost portion, hydrated salt in the heat storage protection film serves as a phase change component and can improve the heat storage performance of the heat storage coating, the heat insulation fiber is arranged between the heat storage protection film and the wind power blade, the flexible organic silicon aerogel composite fiber layer is adopted, heat can be effectively insulated, and the heat storage performance between the wind power blade and the heat insulation fiber is improved. The thermal insulation fiber and the thermal storage protective film are bonded through the bonding coating, and the structure and composition of the protective film can effectively absorb light and heat in the daytime and store the light and heat in the coating, so that the wind power blade is prevented from being frozen after the temperature is reduced at night.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of wind power generation, and in particular relates to a lightning protection, heat storage and ice protection film suitable for the leading edge of a wind power blade and a preparation method thereof. Background Art

[0002] Wind power generation is a clean and renewable energy source, and its core equipment is the wind turbine. Wind turbines are mainly composed of towers, blades, generators, control systems and other parts. Among them, blades are one of the most critical components of wind turbines. Its design and material selection directly affect the performance and service life of wind turbines. However, wind turbines are usually located in high mountains or border areas with large temperature differences between day and night, which are prone to freezing, and these areas often experience extreme weather, such as thunder and lightning weather. These areas have sufficient sunlight and relatively high temperatures during the day, but the temperature drops below zero at night, making the surface of the blades of wind turbines very easy to freeze. Once the blade surface freezes, it not only affects the aerodynamic performance of the blades and reduces the power generation efficiency of the unit, but also causes about 20% to 50% of the power generation loss in areas with severe ice coverage. Lightning strikes may cause blade damage, affect the normal operation of wind turbines, and even cause serious safety accidents. Therefore, how to make the blades able to resist large temperature differences and have the ability to prevent lightning strikes is an urgent problem to be solved in the current field of wind power generation technology. Summary of the invention

[0003] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a lightning protection, heat storage and anti-icing protective film suitable for the leading edge of a wind turbine blade and a preparation method thereof, so as to solve the problem in the prior art that wind turbine blades are difficult to adapt to large temperature differences in the environment and difficult to have lightning protection capabilities at the same time.

[0004] In order to achieve the above object, the present invention adopts the following technical solutions:

[0005] A method for preparing a lightning protection heat storage and anti-icing protective film suitable for the leading edge of a wind turbine blade, the preparation process comprising: coating an adhesive coating on a blade substrate, then laying a heat insulation fiber, then brushing a layer of adhesive coating, placing a heat storage protective film on the adhesive coating, and obtaining an insulating high-conductivity heat storage and anti-icing film after the adhesive coating is dried;

[0006] The thermal insulation fiber is a flexible organosilicon aerogel composite fiber; the flexible organosilicon aerogel composite fiber is composed of organosilicon sol and hollow glass fiber;

[0007] The heat storage protective film is composed of a hydrated salt / SiC composite phase change filler and a water-based polyaspartic acid ester resin cross-linked by a bonding coating, the hydrated salt / SiC composite phase change filler is composed of a eutectic hydrated salt and silicon carbide, and the eutectic hydrated salt is composed of dipotassium hydrogen phosphate hexahydrate and disodium hydrogen phosphate dodecahydrate;

[0008] The bonding coating is a polyurethane modified epoxy resin adhesive added with modified nano boron nitride, and the modified nano boron nitride is boron nitride wrapped with polydopamine.

[0009] A further improvement of the present invention is:

[0010] Preferably, the preparation method of the organosilicon aerogel is:

[0011] (1) mixing silane, water, citric acid, urea and hexadecyltrimethylammonium chloride, and stirring and dissolving them completely to obtain an organosilicon sol;

[0012] (2) The organosilicon sol is poured into a mold with hollow glass fibers placed therein, the hollow glass fibers are completely impregnated with the organosilicon sol, and after oscillation aging, the oscillated aged material is immersed in water, and after alternate washing with isopropanol and n-hexane, it is dried at room temperature and pressure to obtain a flexible organosilicon aerogel composite fiber.

[0013] Preferably, the silane is a mixture of methyltrimethoxysilane, dimethyldimethoxysilane and vinyltrimethoxysilane in a molar ratio of 1:4:0.1:0.08:3.

[0014] Preferably, the preparation process of the bonding coating is: adding the modified nano boron nitride during the preparation process of component A of the polyurethane modified epoxy resin adhesive, mixing component A and component B of the polyurethane modified epoxy resin adhesive, and stirring evenly to obtain the bonding coating.

[0015] Preferably, the preparation process of the modified nano boron nitride is:

[0016] (1) placing a boron nitride raw material in water and stirring at high speed to obtain a boron nitride suspension;

[0017] (2) adding tris(hydroxymethylaminomethane) to water to obtain a tris(hydroxymethylaminomethane) buffer solution, mixing the tris(hydroxymethylaminomethane) buffer solution and the boron nitride suspension, adding polydopamine, stirring, and then adding NaOH to adjust the pH value of the system to 8.5, and stirring to obtain a mixed solution;

[0018] (3) After the mixed solution obtained in step (2) is centrifuged several times, the precipitate in the lower layer is collected and freeze-dried each time to obtain polydopamine-coated boron nitride, which is modified nano boron nitride.

[0019] Preferably, the preparation process of the bonded heat storage protective film is:

[0020] Step 1, after mixing the hydrated salt / SiC composite phase change filler and the silane coupling agent KH550, toluene is added to prepare a mixed system; the mixed system is placed in a constant temperature oil bath filtration pot, nitrogen is introduced for stirring, and after the reaction is completed, vacuum filtration is performed, the vacuum filtration product is subjected to ultrasonic treatment and then vacuum filtered again, the filtration product is washed with N,N-dimethylformamide and then dried to obtain a modified hydrated salt / SiC composite phase change filler powder;

[0021] Step 2, mixing the hydrated salt / SiC composite phase change filler powder and the polyurethane prepolymer, adding the post-chain extender and stirring, and obtaining an insulating, highly thermally conductive, anti-icing dispersion after stirring;

[0022] Step 3, adding dispersant, titanium dioxide, carbon black, anti-settling agent, defoaming agent, leveling agent, light stabilizer, ultraviolet absorber and solvent to the insulating high thermal conductivity anti-icing dispersion in sequence, stirring and dispersing, and obtaining coating A;

[0023] Step 3, mixing coating A and water-based isocyanate to obtain a heat storage coating;

[0024] Step 4, vacuum-infusing the heat storage coating into a film-making mold, and drying it to obtain a heat storage protective film.

[0025] Preferably, in step 1, the preparation process of the hydrated salt / SiC composite phase change filler is:

[0026] (1) mixing dipotassium hydrogen phosphate hexahydrate and disodium hydrogen phosphate dodecahydrate, heating and stirring to obtain a molten eutectic hydrate salt;

[0027] (2) adding insulating thermal conductive filler silicon carbide to the molten eutectic hydrate salt, and stirring to obtain a eutectic hydrate salt / SiC mixture;

[0028] (3) adding aluminum dihydrogen phosphate bonding coating to the eutectic hydrate salt / SiC mixture to obtain a mixture;

[0029] (4) drying the mixture and then sintering it to obtain a sintered product;

[0030] (5) The sintered product is ball-milled to obtain a hydrated salt / SiC composite phase change filler.

[0031] Preferably, in step 2, the preparation process of the polyurethane prepolymer is:

[0032] The dried polyether diol is placed in a container, nitrogen is introduced into the container, the first catalyst and diisocyanate are added after stirring, the hydrophilic chain extender is added after stirring, and a stirring reaction is carried out, the reaction product is cooled, and a neutralizing agent is added for neutralization reaction to obtain a polyurethane prepolymer.

[0033] Preferably, the hydrophilic chain extender is 2,2-dimethylol propionic acid, dimethylol butyric acid or a mixture of the two;

[0034] The first catalyst is one or more of dibutyltin dilaurate, stannous octoate, and dibutyltin oxide.

[0035] A lightning protection, heat storage and ice protection film suitable for the leading edge of a wind turbine blade, prepared by any one of the above preparation methods, comprising:

[0036] Thermal insulation fibers are arranged outside the wind turbine blades;

[0037] A heat storage protective film is arranged outside the heat insulation fiber;

[0038] The heat-insulating fibers and the wind turbine blades are bonded together by an adhesive coating, and the heat-storage protective film and the heat-insulating fibers are bonded together by an adhesive coating.

[0039] Compared with the prior art, the present invention has the following beneficial effects:

[0040] The present invention discloses a method for preparing a lightning protection heat storage and ice protection film suitable for the leading edge of a wind turbine blade. The preparation method is to set heat insulation fiber and heat storage protective film from inside to outside on the blade substrate, wherein the heat insulation fiber is a flexible organic silicon aerogel composite fiber, and the heat storage protective film is composed of a hydrated salt / SiC composite phase change filler and an aqueous polyaspartic acid ester resin cross-linked by a bonding coating; the heat storage protective film is at the outermost part, and a hydrated salt is set therein as a phase change component, which has the advantages of high phase change enthalpy value, high energy storage density, large thermal conductivity and low price, etc., which can improve the heat storage performance of the heat storage coating, and can more effectively absorb and store daytime light heat in the coating, so as to avoid ice formation and damage of the wind turbine blade after the temperature drops at night. At the same time, the selection of the material should take into account its influence on the performance and weight of the blade to improve the efficiency of the wind turbine. The heat-insulating fiber is set between the heat storage protective film and the blades. It uses a flexible silicone aerogel composite fiber layer, which can not only effectively bond with the base material (blade substrate) fiberglass (epoxy resin material), but also provide limited heat insulation, so that the heat stored in the heat storage protective film can be kept in the heat storage protective film itself as much as possible, reducing the heat dissipated to the outside. While protecting the blade substrate, it can also keep the heat in the film, effectively absorbing heat during the day, and at night the heat is mainly maintained in the film layer and spread outward. The heat-insulating fiber and the heat storage protective film are bonded by an adhesive coating. The adhesive coating uses a polyurethane modified epoxy resin adhesive coating, which can effectively connect the substrate and the heat storage protective film up and down to increase the bonding force. Boron nitride wrapped in polydopamine is also added to the adhesive coating to further reduce the conductivity of the film and improve the insulation performance.

[0041] Furthermore, the heat storage protective film can effectively utilize the heat from daytime sunlight. When the light is strong, it can be absorbed and quickly stored in the blade coating to prevent the wind turbine blades from being burned under strong light during the day. When the temperature drops at night, the coating can quickly release the heat to ensure that the surface of the wind turbine blades does not freeze when the temperature is low at night. At the same time, it can effectively prevent lightning and ultraviolet light from damaging the blades and improve the safety of wind turbines. Silicon carbide is used as a thermal conductor and supporting material in the heat storage protective film. It has the characteristics of high thermal conductivity, electrical insulation and low cost. When the temperature drops at night, the stored heat can be quickly released to the blade surface to ensure the thermal stability of the blade and prevent ice. The thermal conductivity of silicon carbide is greater than 300W / mK, and the resistivity at room temperature can reach 105~1012Ω·cm. It is not easy to conduct electricity and is an insulating material. It does not chemically react with hydrated salts and has a certain corrosion resistance. Its melting temperature or decomposition temperature is higher than the phase change temperature of the phase change component, ensuring the shape stability and processability of the phase change component, and ensuring the adhesion and reliability of the coating, so that it can maintain good heat absorption and heat release effects even in harsh environments. The heat storage protective film has a uniform and stable state, without problems such as agglomeration, and will not increase the weight of the blades, thereby not affecting the efficiency of the wind turbine. The heat storage coating of the present invention is lighter and more suitable for the blades of wind turbines. The preparation process of the heat storage protective film is simple, and the heat storage cost is low. For areas with large temperature differences between day and night, the cost of blade anti-icing and lightning protection can be reduced, which is beneficial to improving the economic benefits of wind power generation. Compared with the prior art, the heat storage coating of the present invention is more economical.

[0042] Furthermore, in order to ensure that the thickness of the heat storage protective layer on the blade surface is consistent after construction, the material is prefabricated into a heat storage protective film before construction, and the film thickness can be adjusted according to the actual situation of the on-site application. The prefabricated film can ensure uniform thickness, which can reduce the construction difficulty and shorten the construction time compared with the paint brushing construction.

[0043] Furthermore, the heat storage coating of the present invention can also provide additional protection functions, such as corrosion protection, etc., to further improve the service life and performance of the blades.

[0044] Furthermore, compared with other films, the bonding coating uses polyurethane modified epoxy resin adhesive coating, which greatly enhances the bonding strength and avoids the phenomenon of falling off after a period of use.

[0045] Furthermore, adding the modified nano boron nitride during the preparation of component A or component B of the polyurethane modified epoxy resin adhesive can prevent the modified nano boron nitride from being difficult to fully and evenly disperse during the preparation of the polyurethane modified epoxy resin adhesive.

[0046] The present invention also discloses a lightning protection, heat storage and ice protection film suitable for the leading edge of a wind turbine blade. The heat storage film includes a heat insulation fiber arranged outside the wind turbine blade and a heat storage protective film arranged outside the heat insulation fiber; the heat insulation fiber and the wind turbine blade are bonded by an adhesive coating, and the heat storage protective film and the heat insulation fiber are bonded by an adhesive coating. The heat storage protective film can store heat during the day. Compared with active deicing technology, it solves the problem of high investment and operation costs, and does not rely on external heat for deicing. The material embeds high thermal conductivity materials into a composite matrix to improve the thermal conductivity and thermal stability of the coating. While ensuring ice protection, it protects the blades from being burned by strong light during the day, and does not affect the performance and weight of the blades, thereby improving the efficiency and stability of the wind turbine set; without increasing the weight, it ensures that the blades have strong insulation and provides lightning protection for the blades. Using silane coupling agent as bonding coating can covalently react with the surface of inorganic materials under certain conditions to form covalent bonds, so that it can firmly exist on the surface of inorganic materials. The amino group in the other section can also covalently react with the polymer collectively to enhance the connection between the supporting material and the polymer matrix, and accordingly improve the overall thermal conductivity of the coating.

[0047] Furthermore, the formula of the heat storage coating was optimized, lower-priced raw materials were selected, and the production process was simplified to reduce the manufacturing cost of the heat storage coating.

[0048] Furthermore, the thermal insulation fiber and the heat storage protection are bonded by adhesive coating, and the fiber adopts flexible silicone aerogel composite fiber, and the countless cavities in the unique hollow structure of the aerogel are used to form a thermal insulation layer to prevent heat conduction. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] Figure 1 It is a schematic diagram of the structure of the insulating high-conductivity heat storage anti-icing film of the present invention. DETAILED DESCRIPTION

[0050] The first aspect of the present invention discloses a method for preparing a lightning protection, heat storage and ice protection film suitable for the leading edge of a wind turbine blade, comprising the following steps:

[0051] Adhesive coating is applied on the blade substrate, and then thermal insulation fiber is laid, and then another layer of adhesive coating is applied, and finally a heat storage protective film is bonded thereon.

[0052] In some embodiments of the present invention, the blade substrate is polished before the adhesive coating is applied, so that impurities on the surface of the blade substrate can be reduced, so that the adhesive coating can be better bonded to the blade surface.

[0053] In some embodiments of the present invention, the adhesive coating is an epoxy resin coating, more specifically a polyurethane modified epoxy resin adhesive, to which modified nano boron nitride is added; polyurethane elastic molecules are introduced into the epoxy resin, and under the action of a curing agent and a catalyst, the two can form an interpenetrating network system IPN, which effectively improves the strength and deformation capacity of the epoxy system, and can serve as a bridge between the epoxy resin substrate and the polyurethane system heat storage protective film.

[0054] Polyurethane modified epoxy resin adhesive is composed of epoxy resin, polyurethane prepolymer (or toughening agent), curing agent, accelerator, filler and other possible additives.

[0055] Specifically, the preparation process of the polyurethane with modified nano boron nitride is as follows: epoxy resin, filler and other raw materials are mixed evenly according to the formula; as component A, curing agent, accelerator and other raw materials are mixed evenly; as component B, A, B components and toughening agent are mixed evenly in a certain proportion; after stirring evenly, a polyurethane modified epoxy resin adhesive can be made; it is necessary to avoid mixing the A combination and the B component in advance to avoid premature curing; in the process of preparing the A component, a set amount of modified nano boron nitride polyurethane can be added, and finally a polyurethane modified epoxy resin adhesive with modified nano boron nitride is formed.

[0056] As a preferred solution, the amount of modified nano boron nitride added to the polyurethane modified epoxy resin adhesive is 3-5wt% of its mass, and the modified nano boron nitride is polydopamine-wrapped boron nitride. The material uses polydopamine to wrap the boron nitride material, and forms a layer of polydopamine film on the surface of the boron nitride material to promote the dispersion of the boron nitride material in the epoxy resin and improve the interface compatibility between the boron nitride and the epoxy resin.

[0057] The specific preparation process of modified nano boron nitride is:

[0058] Step 1, weighing a boron nitride raw material, adding it into deionized water, and stirring it with a high-speed stirrer at 12000-15000 rpm for 8-10 minutes to form a boron nitride suspension, wherein the concentration of the boron nitride suspension is 100 g / mL.

[0059] Step 2, adding tris(hydroxymethylaminomethane) to deionized water to prepare a 0.06 mol / L buffer solution, adding the stirred boron nitride suspension thereto, then adding polydopamine, stirring at 700 rpm after mixing, adding NaOH powder to adjust the pH value to 8.5, and stirring the obtained solution at 700 rpm for 24 hours to obtain a mixed solution; wherein the volume ratio of tris(hydroxymethylaminomethane) buffer solution to the boron nitride suspension is 4:1, and the concentration of polydopamine in the mixed solution is 7.5 g / L.

[0060] Step 3, centrifuging the solution obtained in step 2 at 7000 rpm for 10 times, performing lower layer precipitation each time, and freeze-drying the obtained powder for 24 hours to obtain polydopamine-coated boron nitride (BN-HPDA).

[0061] In some embodiments of the present invention, the thermal insulation fiber is a flexible organic silicon aerogel composite fiber. Combining the ablation heat protection of traditional organic silicon resin and the excellent thermal insulation performance of aerogel, an organic silicon aerogel composite fiber material is prepared.

[0062] The specific preparation method comprises the following steps:

[0063] Step 1, silane, water, citric acid, urea, and hexadecyltrimethylammonium chloride are uniformly mixed in a molar ratio of 1:4:0.1:0.08:3, wherein the silane is a mixture of methyltrimethoxysilane, dimethyldimethoxysilane, and vinyltrimethoxysilane in a molar ratio of 3:5:2.4, and after being completely dissolved, the mixture is vigorously stirred for 0.5 to 1 hour to obtain an organic silica sol.

[0064] Step 2: Pour the organosilicon sol into a mold containing hollow glass fibers of set size to completely impregnate the fibers, place them in an 80°C environment for gel oscillation aging for 24 hours, then soak them in 60°C water for 24 hours, then wash them alternately with 60°C isopropanol and n-hexane solutions twice, each time with an interval of 8 hours, and finally dry them at room temperature and pressure for 72 hours to obtain flexible organosilicon aerogel composite fibers. The obtained flexible organosilicon aerogel composite material is a soft solid material, and the specific thickness and size can be adjusted by adjusting the size of the mold.

[0065] In some embodiments of the present invention, a method for preparing a heat storage protective film is also disclosed. The preparation method uses dipotassium hydrogen phosphate hexahydrate as a phase change matrix, disodium hydrogen phosphate dodecahydrate as a nucleating agent, silicon carbide as a thermal conductor and supporting material, and an aqueous polyaspartic acid resin. Among them, dipotassium hydrogen phosphate hexahydrate, disodium hydrogen phosphate dodecahydrate, and glycine are used together to prepare a eutectic hydrate salt, and a mixed sintering method is used to prepare a hydrated eutectic salt / SiC phase change filler. The hydrated eutectic salt / SiC and the aqueous polyaspartic acid resin are cross-linked and mixed with a binder to form a heat storage coating. The preparation method of the heat storage protective film includes the following steps:

[0066] Step 1, preparation of hydrated salt phase change material

[0067] Dipotassium hydrogen phosphate hexahydrate and disodium hydrogen phosphate dodecahydrate were mixed in a beaker at a mass ratio of 176.67:13.86:0.99, and heated and stirred in a water bath at 55° C. until they melted into a transparent liquid to obtain a molten eutectic hydrate salt.

[0068] Step 2: Preparation of hydrated salt / SiC composite phase change thermal storage material

[0069] (1) Adding insulating thermal conductive filler silicon carbide to the molten eutectic hydrate salt in step 1. After mechanical stirring and mixing for 10 to 15 minutes, a eutectic hydrate salt / SiC mixture is obtained. The stirring speed is 60 to 110 r / min, and the silicon carbide particle size is 2 to 5 μm.

[0070] The mass fraction of the silicon carbide is 50% to 80% of the mass of the eutectic hydrate salt.

[0071] (2) The eutectic hydrate salt / SiC mixture after being fully and evenly mixed is placed in a crucible, and an appropriate amount of aluminum dihydrogen phosphate binder is dropped into it;

[0072] The content of aluminum dihydrogen phosphate is 3-4.5% of the mass of the eutectic hydrated salt / SiC mixture. In the process, aluminum dihydrogen phosphate acts as a binder to bond SiC and eutectic salt particles together.

[0073] (3) The crucible in step (2) is placed in a drying oven at 120° C. for pre-drying for 4 to 6 hours, and then the drying oven is closed and the crucible is taken out after the oven is naturally cooled to room temperature.

[0074] (4) The crucible cooled in step (3) is taken out and sintered according to a specific temperature rising program.

[0075] The heating program is as follows: heating at 0-25°C for 40 minutes and keeping warm for 20 minutes; heating from 25°C to 50°C within 40 minutes and keeping warm at 50°C for 20 minutes; heating from 50°C to 75°C within 40 minutes and keeping warm at 75°C for 20 minutes; heating from 75°C to 100°C within 30 minutes and keeping warm at 100°C for 30 minutes; keeping warm at the highest sintering temperature of 100°C for 1 hour.

[0076] It should be noted that in the above-mentioned heating process, after the process mixture B is taken out, if the temperature of the process mixture B itself is relatively high, there is no need to perform a heating process of 0 to 25° C., and the temperature can be directly increased within the subsequent temperature range.

[0077] (5) After the heat preservation process in step (4) is completed, the mixture in the crucible is taken out and placed in a planetary ball mill. The mixture is dry-milled at a ball-to-material ratio of 1:1 and a speed of 100 r / min until the particle size of the mixture is 10 to 20 μm, thereby obtaining a hydrated salt / SiC composite phase change filler.

[0078] Step 3, weighing the base material of waterborne polyaspartic acid ester resin

[0079] The base materials of the waterborne polyaspartic acid ester resin include: diisocyanate, polyether diol, post-chain extender, hydrophilic chain extender, catalyst, neutralizer and solvent.

[0080] Specifically, the diisocyanate is a mixture of any one or more of isophorone diisocyanate, hexamethylene diisocyanate, and 4,4'-dicyclohexylmethane diisocyanate, and the mass content thereof is 20-25% of the polyurethane base material;

[0081] Specifically, the polyether diol is a mixture of one or more of polytetramethylene glycol (PTMG), polyethylene glycol, and polypropylene glycol, and its mass content is 15-20% of the polyurethane base material;

[0082] Specifically, the post-chain extender is 1,5-pentanediol, and its mass content is 2.5-7.5% of the polyurethane base material;

[0083] Specifically, the hydrophilic chain extender is one or a mixture of 2,2-dimethylol propionic acid and dimethylol butyric acid, and its mass content is 1-2% of the polyurethane base material;

[0084] Specifically, the first catalyst is one or more of dibutyltin dilaurate, stannous octoate, and dibutyltin oxide, and its mass content is 1 to 3.5% of the polyurethane base material;

[0085] Specifically, the neutralizing agent is one or more of triethylamine, tripropylamine, formic acid, acetic acid, and triethanolamine, and its mass content is 0.5-2% of the polyurethane base material.

[0086] Specifically, the solvent is N,N-dimethylformamide, and its mass content is 50% of the polyurethane base material.

[0087] It should be understood that the above polyurethane base material is the composition and corresponding materials of the final water-based polyaspartic acid ester resin, a part of which is used for preparing the polyurethane prepolymer in the next step, and a part of which is added in the final preparation step.

[0088] Step 4: Preparation of polyurethane prepolymer

[0089] (1) Weighing the diisocyanate, the polyether diol, the hydrophilic chain extender, the first catalyst and the neutralizer respectively according to a set mass ratio;

[0090] (2) Dry the weighed polyether diol at 110°C for 5 h.

[0091] (3) The polyether diol dried in step (2) was taken out and added into a three-necked round-bottom flask. Nitrogen was introduced into the flask and stirring was started. The stirring conditions were: 350 r / min for 20 min.

[0092] (4) Add the weighed first catalyst and diisocyanate into the flask of step (3), start stirring, and the stirring conditions are: 350 r / min, 88°C, 30 to 60 min.

[0093] (5) Add the weighed hydrophilic chain extender into the flask of step (4) and start stirring at 350 r / min, 80° C., for 2 to 3 h;

[0094] (6) The reaction product of step (5) is cooled to 50° C., and a weighed neutralizing agent is added to carry out a neutralization reaction for 30 to 40 minutes to obtain a polyurethane prepolymer.

[0095] Step 5: Preparation of insulating high thermal conductivity anti-icing coating

[0096] (1) Hydrated salt / SiC composite phase change filler powder and silane coupling agent KH550 were added into a three-necked flask at a molar ratio of 25:1, and toluene was added as a reaction environment solvent.

[0097] (2) Place the three-necked flask in a constant temperature oil bath, raise the temperature to 90°C, introduce nitrogen and maintain the nitrogen atmosphere, start stirring and react for 6 hours at a stirring speed of 100-150 r / min.

[0098] (3) After the reaction is completed, the mixed solution in (2) is vacuum filtered.

[0099] (4) After vacuum filtration, the hydrated salt / SiC composite phase change filler powder is poured into a beaker, deionized water is added, and ultrasonic treatment is performed for 30 to 60 minutes, followed by filtration again after ultrasonic treatment.

[0100] (5) Add N,N-dimethylformamide to the hydrated salt / SiC composite phase change filler powder filtered in (4) and wash it twice.

[0101] (6) The cleaned hydrated salt / SiC composite phase change filler powder in (5) is placed in a vacuum drying oven; the drying oven needs to be heated to 105° C. in advance and kept at a constant temperature for 12 hours to obtain the modified hydrated salt / SiC composite phase change filler powder.

[0102] (7) The reaction product of step (6) is cooled to 35° C. and added to the polyurethane prepolymer in an amount of 30 to 60% by mass of the polyurethane prepolymer.

[0103] (8) The weighed post-chain extender and solvent are added to (7), and stirring is started at 900-2000 r / min for 30-60 min to finally obtain an insulating, highly thermally conductive, anti-icing dispersion.

[0104] (9) Add dispersant (accounting for 1% to 1.5% of the total mass fraction of component A, acrylic dispersant), titanium dioxide (accounting for 25% to 30% of component A, filler for coloring), carbon black (accounting for 0.05% to 0.1% of component A, for coloring and enhancing light absorption), anti-settling agent (accounting for 0.5% to 1% of component A, nano-silicon dioxide or polyamide wax), defoamer (0.5% to 1%), leveling agent (0.8% to 1%), light stabilizer (0.5% to 1%, a mixture of bis(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate and 1-methyl-8-(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate), ultraviolet absorber (0.8% to 1.2%, hydroxyphenylbenzotriazole ultraviolet absorber), and solvent (propylene glycol methyl ether acetate, dimethyl sulfoxide, xylene, 3% to 10%) in sequence to the dispersion obtained in step (8). After adding and mixing them uniformly at a low speed, high-speed dispersion is carried out at 2500rpm / min, keeping the temperature above 40 degrees for not less than 30 minutes, and the detected fineness is not higher than 50μm, to form coating A.

[0105] In the coating component A, in terms of mass fraction, in addition to the above-mentioned dispersant, titanium dioxide, carbon black, anti-settling agent, defoaming agent, leveling agent, light stabilizer, ultraviolet absorber and solvent, the balance is dispersion.

[0106] (10) According to the weight of the dispersion modified by the reaction product in step (8), the weight of the aqueous isocyanate (component B) is weighed, and the ratio of the two is calculated as n(—NCO):n(—NH)=1.2:1. Before use, component A and component B can be fully stirred and mixed evenly to finally obtain a heat storage coating.

[0107] (11) The heat storage coating is vacuum-infused into a film-making mold. The bottom material of the mold is a polytetrafluoroethylene substrate, which is non-adhesive. The thickness of the infusion is controlled to be 200 μm to 500 μm. After being placed for 24 hours, the finished heat storage film can be torn off and taken out.

[0108] The following is further described in conjunction with specific embodiments.

[0109] Example 1

[0110] Step 1, preparing a bonding coating;

[0111] The component A of the bonding coating includes epoxy resin E-44 and filler; the component B includes curing agent I, polyamide 650, DMP and toughening agent;

[0112] Epoxy resin E-44, filler and modified nano boron nitride are mixed to obtain component A, and curing agent I, polyamide 650 and DMP are mixed to form component B; component A, component B and toughening agent are mixed and stirred to obtain a bonding coating; wherein the amount of modified nano boron nitride is 3wt% of the mass of the entire bonding coating.

[0113] Step 2, preparing thermal insulation fibers;

[0114] (1) Silane, water, citric acid, urea, and hexadecyltrimethylammonium chloride are uniformly mixed, wherein the silane is a mixture of methyltrimethoxysilane, dimethyldimethoxysilane, and vinyltrimethoxysilane in a molar ratio of 3:5:2.4, and after being completely dissolved, the mixture is vigorously stirred for 1 hour to obtain an organic silica sol.

[0115] (2) The organosilicon sol is poured into a mold containing hollow glass fibers of the same size to completely impregnate the fibers, and then placed in an 80°C environment for gel oscillation aging for 24 hours, then soaked in 60°C water for 24 hours, and then washed twice with 60°C isopropanol and n-hexane solutions alternately, each time with an interval of 8 hours, and finally dried at room temperature and pressure for 72 hours to obtain a flexible organosilicon aerogel composite fiber. The obtained flexible organosilicon aerogel composite material is a soft solid material, and the specific thickness and size can be adjusted by adjusting the size of the mold.

[0116] Step 3: Preparation of heat storage protective film

[0117] Step 3.1, Preparation of hydrated salt phase change material

[0118] Dipotassium hydrogen phosphate hexahydrate and disodium hydrogen phosphate dodecahydrate were mixed in a beaker at a mass ratio of 176.67:13.86, and heated and stirred in a water bath at 55° C. until they melted into a transparent liquid to obtain a molten eutectic hydrated salt.

[0119] Step 3.2, preparation of hydrated salt / SiC composite phase change thermal storage material

[0120] (1) Adding insulating thermal conductive filler silicon carbide to the molten eutectic hydrate salt obtained in step 3.1. After mechanical stirring and mixing for 12 minutes, a eutectic hydrate salt / SiC mixture is obtained. The stirring speed is 80 r / min, and the silicon carbide particle size is 2 to 5 μm.

[0121] The mass fraction of the silicon carbide is 60% of the mass of the eutectic hydrate salt.

[0122] (2) The eutectic hydrate salt / SiC mixture after being fully and evenly mixed is placed in a crucible, and an appropriate amount of aluminum dihydrogen phosphate binder is dropped into it to obtain a process mixture A;

[0123] The content of aluminum dihydrogen phosphate is 4% of the mass of the eutectic hydrate salt / SiC mixture.

[0124] (3) placing the process mixture A obtained in step (2) in a crucible, placing the crucible in a drying oven at 120° C. and drying for 5 h, then closing the drying oven, and taking out the crucible after the oven is naturally cooled to room temperature, thereby obtaining a process mixture B;

[0125] (4) taking out the cooled process mixture B and sintering it at a specific temperature rising program to obtain process mixture C;

[0126] The heating program is as follows: heating from room temperature to 30°C, heating for 40 minutes, and keeping warm for 20 minutes; heating to 60°C, heating for 40 minutes, and keeping warm for 20 minutes; heating to 90°C, heating for 30 minutes, and keeping warm for 30 minutes; keeping warm at the highest sintering temperature of 100°C for 1 hour.

[0127] (5) After the heat preservation process in step (4) is completed, the process mixture C in the crucible is taken out and placed in a planetary ball mill. The mixture is dry-milled at a ball-to-material ratio of 1:1 and a speed of 100 r / min until the particle size of the mixture is 10 to 20 μm, thereby obtaining a hydrated salt / SiC composite phase change filler.

[0128] Step 3.3, weighing the polyurethane base

[0129] Specifically, the diisocyanate is isophorone diisocyanate, and its mass content is 22% of the polyurethane base material;

[0130] Specifically, the polyether diol is polytetrahydrofuran diol, and its mass content is 18% of the polyurethane prepolymer;

[0131] Specifically, the post-chain extender is 1,5-pentanediol, and its mass content is 5% of the polyurethane prepolymer;

[0132] Specifically, the hydrophilic chain extender is 2,2-dimethylol propionic acid, and its mass content is 1.5% of the polyurethane prepolymer;

[0133] Specifically, the catalyst is dibutyltin dilaurate, and its mass content is 2% of the polyurethane prepolymer;

[0134] Specifically, the neutralizing agent is a type of triethylamine, and its mass content is 1.5% of the polyurethane prepolymer.

[0135] Specifically, the solvent is N,N-dimethylformamide, and its mass content is 50% of the polyurethane prepolymer.

[0136] Step 3.4, preparation of polyurethane prepolymer

[0137] (1) Weighing diisocyanate, polyether diol, post-chain extender, hydrophilic chain extender, catalyst, neutralizer and solvent respectively according to a set mass ratio;

[0138] (2) Dry the weighed polyether diol at 110°C for 5 h.

[0139] (3) The polyether diol dried in step (2) was taken out and added into a three-necked round-bottom flask, nitrogen was introduced into the flask, and stirring was started at a stirring speed of 350 r / min for 20 min.

[0140] (4) Add the weighed catalyst and diisocyanate into the flask of step (3), start stirring, the stirring speed is 350r / min, the stirring temperature is 88°C, and the stirring time is 50min.

[0141] (5) Add the weighed hydrophilic chain extender to the flask of step (4), start stirring, the stirring speed is 350r / min, the stirring temperature is 80°C, and the stirring time is 2.5h;

[0142] (6) The reaction product of step (5) was cooled to 50° C., and a weighed neutralizing agent was added to carry out a neutralization reaction for 35 min to obtain a polyurethane prepolymer.

[0143] Step 3.5, Preparation of modified hydrated salt / SiC composite phase change filler powder

[0144] (1) The hydrated salt / SiC composite phase change filler and the silane coupling agent KH550 were added into a three-necked flask in a ratio of 25:1, and toluene was added as a reaction environment solvent.

[0145] (2) Place the three-necked flask in a constant temperature oil bath, raise the temperature to 90°C, introduce nitrogen and maintain the nitrogen atmosphere, start stirring and react for 6 hours at a stirring speed of 120 r / min.

[0146] (3) After the reaction is completed, the mixed solution in (2) is vacuum filtered.

[0147] (4) After vacuum filtration, the hydrated salt / SiC composite phase change filler powder is poured into a beaker, deionized water is added, and ultrasonic treatment is performed for 40 minutes, followed by filtration again.

[0148] (5) Add N,N-dimethylformamide to the hydrated salt / SiC composite phase change filler powder filtered in (4) and wash it twice.

[0149] (6) The cleaned hydrated salt / SiC composite phase change filler powder in (5) is placed in a vacuum drying oven; the drying oven needs to be heated to 105°C in advance and kept at a constant temperature for 12 hours to obtain the modified hydrated salt / SiC composite phase change filler powder.

[0150] Step 3.6, prepare insulating high thermal conductivity anti-icing coating.

[0151] (1) The reaction product of step 3.5 is cooled to 35° C. and added to the polyurethane prepolymer in an amount of 40% by mass of the polyurethane prepolymer to obtain a mixture.

[0152] (2) Add the weighed post-chain extender and solvent to the mixture obtained in the previous step, and start stirring at 1500 r / min for 40 min to finally obtain an insulating, highly thermally conductive, anti-icing coating.

[0153] Example 2

[0154] Step 1, preparing a bonding coating;

[0155] The component A of the bonding coating includes epoxy resin E-44 and filler; the component B includes curing agent I, polyamide 650, DMP and toughening agent;

[0156] Epoxy resin E-44, filler and modified nano boron nitride are mixed to obtain component A, and curing agent I, polyamide 650 and DMP are mixed to form component B; component A, component B and toughening agent are mixed and stirred to obtain bonding coating; wherein the amount of modified nano boron nitride is 4wt% of the mass of the whole bonding coating.

[0157] Step 2, preparing thermal insulation fibers;

[0158] (1) Silane, water, citric acid, urea, and hexadecyltrimethylammonium chloride are uniformly mixed, wherein the silane is a mixture of methyltrimethoxysilane, dimethyldimethoxysilane, and vinyltrimethoxysilane in a molar ratio of 3:5:2.4, and after being completely dissolved, the mixture is vigorously stirred for 1 hour to obtain an organic silica sol.

[0159] (2) The organosilicon sol is poured into a mold containing hollow glass fibers of the same size to completely impregnate the fibers, and then placed in an 80°C environment for gel oscillation aging for 24 hours, then soaked in 60°C water for 24 hours, and then washed twice with 60°C isopropanol and n-hexane solutions alternately, each time with an interval of 8 hours, and finally dried at room temperature and pressure for 72 hours to obtain a flexible organosilicon aerogel composite fiber. The obtained flexible organosilicon aerogel composite material is a soft solid material, and the specific thickness and size can be adjusted by adjusting the size of the mold.

[0160] Step 3: Preparation of heat storage protective film

[0161] Step 3.1, Preparation of hydrated salt phase change material

[0162] Dipotassium hydrogen phosphate hexahydrate and disodium hydrogen phosphate dodecahydrate were mixed in a beaker at a mass ratio of 176.67:13.86, and heated and stirred in a water bath at 55° C. until they melted into a transparent liquid to obtain a eutectic hydrated salt.

[0163] Step 3.2, preparation of hydrated salt / SiC composite phase change thermal storage material

[0164] (1) Adding insulating thermal conductive filler silicon carbide to the molten eutectic hydrate salt obtained in step 1. After mechanical stirring and mixing for 10 minutes, a eutectic hydrate salt / SiC mixture is obtained. The stirring speed is 110 r / min, and the silicon carbide particle size is 2 to 5 μm.

[0165] The mass fraction of the silicon carbide is 50% of the mass of the eutectic hydrated salt.

[0166] (2) The eutectic hydrate salt / SiC mixture after being fully and evenly mixed is placed in a crucible, and an appropriate amount of aluminum dihydrogen phosphate binder is dropped into it to obtain a process mixture A;

[0167] The content of aluminum dihydrogen phosphate is 3% of the mass of the eutectic hydrate salt / SiC mixture.

[0168] (3) placing the process mixture A obtained in step (3) in a crucible, placing the crucible in a drying oven at 120° C. and drying for 4 h, then closing the drying oven, and taking out the crucible after the oven is naturally cooled to room temperature, thereby obtaining a process mixture B;

[0169] (4) taking out the cooled process mixture B and sintering it at a specific temperature rising program to obtain process mixture C;

[0170] The heating program is as follows: heating from room temperature to 25°C, heating for 40 minutes, and keeping warm for 20 minutes; heating to 50°C, heating for 40 minutes, and keeping warm for 20 minutes; heating to 75°C, heating for 30 minutes, and keeping warm for 30 minutes; keeping warm at the highest sintering temperature of 100°C for 1 hour.

[0171] (5) After the heat preservation process in step (4) is completed, the process mixture C in the crucible is taken out and placed in a planetary ball mill. The mixture is dry-milled at a ball-to-material ratio of 1:1 and a speed of 100 r / min until the particle size of the mixture is 10 to 20 μm, thereby obtaining a hydrated salt / SiC composite phase change filler.

[0172] Step 3.3, weighing the polyurethane base

[0173] Specifically, the diisocyanate is hexamethylene diisocyanate, and its mass content is 20% of the polyurethane base material;

[0174] Specifically, the polyether diol is polyethylene glycol, and its mass content is 20% of the polyurethane prepolymer;

[0175] Specifically, the post-chain extender is 1,5-pentanediol, and its mass content is 4% of the polyurethane prepolymer;

[0176] Specifically, the hydrophilic chain extender is dimethylolbutyric acid, and its mass content is 2% of the polyurethane prepolymer;

[0177] Specifically, the catalyst is stannous octoate, and its mass content is 2% of the polyurethane prepolymer;

[0178] Specifically, the neutralizing agent is formic acid, and its mass content is 2% of the polyurethane prepolymer.

[0179] Specifically, the solvent is N,N-dimethylformamide, and its mass content is 50% of the polyurethane prepolymer.

[0180] Step 3.4, preparation of polyurethane prepolymer

[0181] (1) Weighing diisocyanate, polyether diol, post-chain extender, hydrophilic chain extender, catalyst, neutralizer and solvent respectively according to a set mass ratio;

[0182] (2) Dry the weighed polyether diol at 110°C for 5 h.

[0183] (3) The polyether diol dried in step (2) was taken out and added into a three-necked round-bottom flask, nitrogen was introduced into the flask, and stirring was started at a stirring speed of 350 r / min for 20 min.

[0184] (4) Add the weighed catalyst and diisocyanate into the flask of step (3), start stirring, the stirring speed is 350r / min, the stirring temperature is 88°C, and the stirring time is 30min.

[0185] (5) Add the weighed hydrophilic chain extender to the flask of step (4), start stirring, the stirring speed is 350r / min, the stirring temperature is 80°C, and the stirring time is 2h;

[0186] (6) The reaction product of step (5) was cooled to 50° C., and a weighed neutralizing agent was added to carry out a neutralization reaction for 30 min to obtain a polyurethane prepolymer.

[0187] Step 3.5, Preparation of modified hydrated salt / SiC composite phase change filler powder

[0188] (1) The hydrated salt / SiC composite phase change filler and the silane coupling agent KH550 were added into a three-necked flask in a ratio of 25:1, and toluene was added as a reaction environment solvent.

[0189] (2) Place the three-necked flask in a constant temperature oil bath, raise the temperature to 90°C, introduce nitrogen and maintain the nitrogen atmosphere, start stirring and react for 6 hours at a stirring speed of 100 r / min.

[0190] (3) After the reaction is completed, the mixed solution in (2) is vacuum filtered.

[0191] (4) After vacuum filtration, the hydrated salt / SiC composite phase change filler powder is poured into a beaker, deionized water is added, and ultrasonic treatment is performed for 30 minutes, followed by filtration again.

[0192] (5) Add N,N-dimethylformamide to the hydrated salt / SiC composite phase change filler powder filtered in (4) and wash it twice.

[0193] (6) The cleaned hydrated salt / SiC composite phase change filler powder in (5) is placed in a vacuum drying oven; the drying oven needs to be heated to 105°C in advance and kept at a constant temperature for 12 hours to obtain the modified hydrated salt / SiC composite phase change filler powder.

[0194] Step 3.6, prepare insulating high thermal conductivity anti-icing coating.

[0195] (1) The reaction product of step 4 is cooled to 35° C. and added into the polyurethane prepolymer in an amount of 40% by mass of the polyurethane prepolymer.

[0196] (2) The weighed post-chain extender and solvent are added to (7), and stirring is started at 900 r / min for 60 min to finally obtain an insulating, highly thermally conductive, anti-icing coating.

[0197] Example 3

[0198] Step 1, preparing a bonding coating;

[0199] The component A of the bonding coating includes epoxy resin E-44 and filler; the component B includes curing agent I, polyamide 650, DMP and toughening agent;

[0200] Epoxy resin E-44, filler and modified nano boron nitride are mixed to obtain component A, and curing agent I, polyamide 650 and DMP are mixed to form component B; component A, component B and toughening agent are mixed and stirred to obtain a bonding coating; wherein the amount of modified nano boron nitride is 5wt% of the mass of the entire bonding coating.

[0201] Step 2, preparing thermal insulation fibers;

[0202] (1) Silane, water, citric acid, urea, and hexadecyltrimethylammonium chloride are uniformly mixed, wherein the silane is a mixture of methyltrimethoxysilane, dimethyldimethoxysilane, and vinyltrimethoxysilane in a molar ratio of 3:5:2.4, and after being completely dissolved, the mixture is vigorously stirred for 1 hour to obtain an organic silica sol.

[0203] (2) The organosilicon sol is poured into a mold containing hollow glass fibers of the same size to completely impregnate the fibers, and then placed in an 80°C environment for gel oscillation aging for 24 hours, then soaked in 60°C water for 24 hours, and then washed twice with 60°C isopropanol and n-hexane solutions alternately, each time with an interval of 8 hours, and finally dried at room temperature and pressure for 72 hours to obtain a flexible organosilicon aerogel composite fiber. The obtained flexible organosilicon aerogel composite material is a soft solid material, and the specific thickness and size can be adjusted by adjusting the size of the mold.

[0204] Step 3: Preparation of heat storage protective film

[0205] Step 3.1, Preparation of hydrated salt phase change material

[0206] Dipotassium hydrogen phosphate hexahydrate and disodium hydrogen phosphate dodecahydrate were mixed in a beaker at a mass ratio of 176.67:13.86, and heated and stirred in a water bath at 55° C. until they melted into a transparent liquid to obtain a molten eutectic hydrated salt.

[0207] Step 3.2, preparation of hydrated salt / SiC composite phase change thermal storage material

[0208] (1) Adding insulating thermal conductive filler silicon carbide to the molten eutectic hydrate salt obtained in step 3.1. After mechanical stirring and mixing for 15 minutes, a eutectic hydrate salt / SiC mixture is obtained. The stirring speed is 60 r / min, and the silicon carbide particle size is 2 to 5 μm.

[0209] The mass fraction of the silicon carbide is 80% of the mass of the eutectic hydrate salt.

[0210] (2) The eutectic hydrate salt / SiC mixture after being fully and evenly mixed is placed in a crucible, and an appropriate amount of aluminum dihydrogen phosphate binder is dropped into it to obtain a process mixture A;

[0211] The content of aluminum dihydrogen phosphate is 4.5% of the mass of the eutectic hydrate salt / SiC mixture.

[0212] (3) placing the process mixture A obtained in step (2) in a crucible, placing the crucible in a drying oven at 120° C. and drying for 6 h, then closing the drying oven, and taking out the crucible after the oven is naturally cooled to room temperature, thereby obtaining a process mixture B;

[0213] (4) taking out the cooled process mixture B and sintering it at a specific temperature rising program to obtain process mixture C;

[0214] The heating program is as follows: heating from room temperature to 50°C, heating for 40 minutes, and keeping warm for 20 minutes; heating to 75°C, heating for 40 minutes, and keeping warm for 20 minutes; heating to 100°C, heating for 30 minutes, and keeping warm for 30 minutes; keeping warm at the highest sintering temperature of 100°C for 1 hour.

[0215] (5) After the heat preservation process in step (4) is completed, the process mixture C in the crucible is taken out and placed in a planetary ball mill. The mixture is dry-milled at a ball-to-material ratio of 1:1 and a speed of 100 r / min until the particle size of the mixture is 10 to 20 μm, thereby obtaining a hydrated salt / SiC composite phase change filler.

[0216] Step 3.3, weighing the polyurethane base

[0217] Specifically, the diisocyanate is 4,4'-dicyclohexylmethane diisocyanate, and its mass content is 25% of the polyurethane base material;

[0218] Specifically, the polyether diol is polypropylene glycol, and its mass content is 15% of the polyurethane prepolymer;

[0219] Specifically, the post-chain extender is 1,5-pentanediol, and its mass content is 2.5% of the polyurethane prepolymer;

[0220] Specifically, the hydrophilic chain extender is 2,2-dimethylol propionic acid, and its mass content is 2% of the polyurethane prepolymer;

[0221] Specifically, the catalyst is dibutyltin oxide, and its mass content is 3.5% of the polyurethane prepolymer;

[0222] Specifically, the neutralizing agent is triethanolamine, and its mass content is 2% of the polyurethane prepolymer.

[0223] Specifically, the solvent is N,N-dimethylformamide, and its mass content is 50% of the polyurethane prepolymer.

[0224] Step 3.4, preparation of polyurethane prepolymer

[0225] (1) Weighing diisocyanate, polyether diol, post-chain extender, hydrophilic chain extender, catalyst, neutralizer and solvent respectively according to a set mass ratio;

[0226] (2) Dry the weighed polyether diol at 110°C for 5 h.

[0227] (3) The polyether diol dried in step (2) was taken out and added into a three-necked round-bottom flask, nitrogen was introduced into the flask, and stirring was started at a stirring speed of 350 r / min for 20 min.

[0228] (4) Add the weighed catalyst and diisocyanate into the flask of step (3), start stirring, the stirring speed is 350r / min, the stirring temperature is 88°C, and the stirring time is 60min.

[0229] (5) Add the weighed hydrophilic chain extender to the flask of step (4), start stirring, the stirring speed is 350r / min, the stirring temperature is 80°C, and the stirring time is 3h;

[0230] (6) The reaction product of step (5) was cooled to 50° C., and a weighed neutralizing agent was added to carry out a neutralization reaction for 40 minutes to obtain a polyurethane prepolymer.

[0231] Step 3.5, Preparation of modified hydrated salt / SiC composite phase change filler powder

[0232] (1) The hydrated salt / SiC composite phase change filler and the silane coupling agent KH550 were added into a three-necked flask in a ratio of 25:1, and toluene was added as a reaction environment solvent.

[0233] (2) Place the three-necked flask in a constant temperature oil bath, raise the temperature to 90°C, introduce nitrogen and maintain the nitrogen atmosphere, start stirring and react for 6 hours at a stirring speed of 150 r / min.

[0234] (3) After the reaction is completed, the mixed solution in step (2) is vacuum filtered.

[0235] (4) After vacuum filtration, the hydrated salt / SiC composite phase change filler powder is poured into a beaker, deionized water is added, and ultrasonic treatment is performed for 60 minutes. After ultrasonic treatment, the powder is filtered again.

[0236] (5) Add N,N-dimethylformamide to the hydrated salt / SiC composite phase change filler powder filtered in step (4) and wash it twice.

[0237] (6) Place the cleaned hydrated salt / SiC composite phase change filler powder in step (5) into a vacuum drying oven; the drying oven needs to be heated to 105° C. in advance and kept at a constant temperature for 12 hours to obtain the modified hydrated salt / SiC composite phase change filler powder.

[0238] Step 3.6, prepare insulating high thermal conductivity anti-icing coating.

[0239] (1) The reaction product of step 3.5 is cooled to 35° C. and added to the polyurethane prepolymer in an amount of 40% by mass of the polyurethane prepolymer to obtain a mixture.

[0240] (2) Add the weighed post-chain extender and solvent to the mixture obtained in the previous step, and start stirring at a stirring speed of 2000 r / min and a stirring temperature of 30 min to finally obtain an insulating, highly thermally conductive, anti-icing coating.

[0241] Example 4

[0242] Step 1, preparing a bonding coating;

[0243] The component A of the bonding coating includes epoxy resin E-44 and filler; the component B includes curing agent I, polyamide 650, DMP and toughening agent;

[0244] Epoxy resin E-44, filler and modified nano boron nitride are mixed to obtain component A, and curing agent I, polyamide 650 and DMP are mixed to form component B; component A, component B and toughening agent are mixed and stirred to obtain a bonding coating; wherein the amount of modified nano boron nitride is 3wt% of the mass of the entire bonding coating.

[0245] Step 2, preparing thermal insulation fibers;

[0246] (1) Silane, water, citric acid, urea, and hexadecyltrimethylammonium chloride are uniformly mixed, wherein the silane is a mixture of methyltrimethoxysilane, dimethyldimethoxysilane, and vinyltrimethoxysilane in a molar ratio of 3:5:2.4, and after being completely dissolved, the mixture is vigorously stirred for 1 hour to obtain an organic silica sol.

[0247] (2) The organosilicon sol is poured into a mold containing hollow glass fibers of the same size to completely impregnate the fibers, and then placed in an 80°C environment for gel oscillation aging for 24 hours, then soaked in 60°C water for 24 hours, and then washed twice with 60°C isopropanol and n-hexane solutions alternately, each time with an interval of 8 hours, and finally dried at room temperature and pressure for 72 hours to obtain a flexible organosilicon aerogel composite fiber. The obtained flexible organosilicon aerogel composite material is a soft solid material, and the specific thickness and size can be adjusted by adjusting the size of the mold.

[0248] Step 3: Preparation of heat storage protective film

[0249] Step 3.1, Preparation of hydrated salt phase change material

[0250] Dipotassium hydrogen phosphate hexahydrate and disodium hydrogen phosphate dodecahydrate were mixed in a beaker at a mass ratio of 176.67:13.86, and heated and stirred in a water bath at 55° C. until they melted into a transparent liquid to obtain a eutectic hydrated salt.

[0251] Step 3.2, preparation of hydrated salt / SiC composite phase change thermal storage material

[0252] (1) Adding insulating thermal conductive filler silicon carbide to the molten eutectic hydrate salt obtained in step 3.1. After mechanical stirring and mixing for 13 minutes, a eutectic hydrate salt / SiC mixture is obtained. The stirring speed is 100 r / min, and the silicon carbide particle size is 2 to 5 μm.

[0253] The mass fraction of the silicon carbide is 70% of the mass of the eutectic hydrate salt.

[0254] (2) The eutectic hydrate salt / SiC mixture after being fully and evenly mixed is placed in a crucible, and an appropriate amount of aluminum dihydrogen phosphate binder is dropped into it to obtain a process mixture A;

[0255] The content of aluminum dihydrogen phosphate is 3.5% of the mass of the eutectic hydrate salt / SiC mixture.

[0256] (3) placing the process mixture A obtained in step (2) in a crucible, placing the crucible in a drying oven at 120° C. and drying for 6 h, then closing the drying oven, and taking out the crucible after the oven is naturally cooled to room temperature, thereby obtaining a process mixture B;

[0257] (4) taking out the cooled process mixture B and sintering it at a specific temperature rising program to obtain process mixture C;

[0258] The heating program is as follows: heating from room temperature to 40°C, heating for 40 minutes, and keeping warm for 20 minutes; heating to 70°C, heating for 40 minutes, and keeping warm for 20 minutes; heating to 80°C, heating for 30 minutes, and keeping warm for 30 minutes; keeping warm at the highest sintering temperature of 100°C for 1 hour.

[0259] (5) After the heat preservation process in step (4) is completed, the process mixture C in the crucible is taken out and placed in a planetary ball mill. The mixture is dry-milled at a ball-to-material ratio of 1:1 and a speed of 100 r / min until the particle size of the mixture is 10 to 20 μm, thereby obtaining a hydrated salt / SiC composite phase change filler.

[0260] Step 3.3, weighing polyurethane pre-base

[0261] Specifically, the diisocyanate is isophorone diisocyanate, and its mass content is 23% of the polyurethane base material;

[0262] Specifically, the polyether diol is polytetrahydrofuran diol, and its mass content is 17% of the polyurethane prepolymer;

[0263] Specifically, the post-chain extender is 1,5-pentanediol, and its mass content is 7.5% of the polyurethane prepolymer;

[0264] Specifically, the hydrophilic chain extender is 2,2-dimethylol propionic acid, and its mass content is 1% of the polyurethane prepolymer;

[0265] Specifically, the catalyst is dibutyltin dilaurate, and its mass content is 1% of the polyurethane prepolymer;

[0266] Specifically, the neutralizing agent is tripropylamine, and its mass content is 0.5% of the polyurethane prepolymer.

[0267] Specifically, the solvent is N,N-dimethylformamide, and its mass content is 50% of the polyurethane prepolymer.

[0268] Step 3.4, preparation of polyurethane prepolymer

[0269] (1) Weighing diisocyanate, polyether diol, post-chain extender, hydrophilic chain extender, catalyst, neutralizer and solvent respectively according to a set mass ratio;

[0270] (2) Dry the weighed polyether diol at 110°C for 5 h.

[0271] (3) The polyether diol dried in step (2) was taken out and added into a three-necked round-bottom flask, nitrogen was introduced into the flask, and stirring was started at a stirring speed of 350 r / min for 20 min.

[0272] (4) Add the weighed catalyst and diisocyanate into the flask of step (3), start stirring, the stirring speed is 350r / min, the stirring temperature is 88°C, and the stirring time is 40min.

[0273] (5) Add the weighed hydrophilic chain extender to the flask of step (4), start stirring, the stirring speed is 350r / min, the stirring temperature is 80°C, and the stirring time is 3h;

[0274] (6) The reaction product of step (5) was cooled to 50° C., and a weighed neutralizing agent was added to carry out a neutralization reaction for 30 min to obtain a polyurethane prepolymer.

[0275] Step 3.5, Preparation of modified hydrated salt / SiC composite phase change filler powder

[0276] (1) The hydrated salt / SiC composite phase change filler and the silane coupling agent KH550 were added into a three-necked flask in a ratio of 25:1, and toluene was added as a reaction environment solvent.

[0277] (2) Place the three-necked flask in a constant temperature oil bath, raise the temperature to 90°C, introduce nitrogen and maintain the nitrogen atmosphere, start stirring and react for 6 hours at a stirring speed of 110 r / min.

[0278] (3) After the reaction is completed, the mixed solution in step (2) is vacuum filtered.

[0279] (4) After vacuum filtration, the hydrated salt / SiC composite phase change filler powder is poured into a beaker, deionized water is added, and ultrasonic treatment is performed for 50 minutes. After ultrasonic treatment, the powder is filtered again.

[0280] (5) Add N,N-dimethylformamide to the hydrated salt / SiC composite phase change filler powder filtered in step (4) and wash it twice.

[0281] (6) Place the cleaned hydrated salt / SiC composite phase change filler powder in step (5) into a vacuum drying oven; the drying oven needs to be heated to 105° C. in advance and kept at a constant temperature for 12 hours to obtain the modified hydrated salt / SiC composite phase change filler powder.

[0282] Step 3.6, prepare insulating high thermal conductivity anti-icing coating.

[0283] (1) The reaction product of step 3.5 is cooled to 35° C. and added to the polyurethane prepolymer in an amount of 40% by mass of the polyurethane prepolymer to obtain a mixture.

[0284] (2) Add the weighed post-chain extender and solvent to the mixture obtained in the previous step, and start stirring at 1500 r / min for 40 min to finally obtain an insulating, highly thermally conductive, anti-icing coating.

[0285] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a lightning protection, heat storage and ice protection film suitable for the leading edge of a wind turbine blade, characterized in that: The preparation process is as follows: coating the blade substrate with adhesive coating, then laying the heat-insulating fiber, then brushing another layer of adhesive coating, placing the heat-storage protective film on the adhesive coating, and obtaining the insulating high-conductivity heat-storage anti-icing film after the adhesive coating dries; The thermal insulation fiber is a flexible organic silicon aerogel composite fiber; The flexible organosilicon aerogel composite fiber is composed of organosilicon sol and hollow glass fiber; The heat storage protective film is composed of a hydrated salt / SiC composite phase change filler and a water-based polyaspartic acid ester resin cross-linked by a bonding coating, the hydrated salt / SiC composite phase change filler is composed of a eutectic hydrated salt and silicon carbide, and the eutectic hydrated salt is composed of dipotassium hydrogen phosphate hexahydrate and disodium hydrogen phosphate dodecahydrate; The bonding coating is a polyurethane modified epoxy resin adhesive added with modified nano boron nitride, and the modified nano boron nitride is boron nitride wrapped with polydopamine.

2. The method for preparing a lightning protection, heat storage and ice protection film suitable for the leading edge of a wind turbine blade according to claim 1, characterized in that: The preparation method of the organosilicon aerogel is: (1) mixing silane, water, citric acid, urea and hexadecyltrimethylammonium chloride, and stirring and dissolving them completely to obtain an organosilicon sol; (2) The organosilicon sol is poured into a mold with hollow glass fibers placed therein, the hollow glass fibers are completely impregnated with the organosilicon sol, and after oscillation aging, the oscillated aged material is immersed in water, and after alternate washing with isopropanol and n-hexane, it is dried at room temperature and pressure to obtain a flexible organosilicon aerogel composite fiber.

3. The method for preparing a lightning protection, heat storage and ice protection film suitable for the leading edge of a wind turbine blade according to claim 2, characterized in that: The silane is a mixture of methyltrimethoxysilane, dimethyldimethoxysilane and vinyltrimethoxysilane in a molar ratio of 1:4:0.1:0.08:

3.

4. The method for preparing a lightning protection, heat storage and ice protection film suitable for the leading edge of a wind turbine blade according to claim 1, characterized in that: The preparation process of the bonding coating is as follows: adding the modified nano boron nitride during the preparation process of component A of the polyurethane modified epoxy resin adhesive, mixing the component A and the component B of the polyurethane modified epoxy resin adhesive, and stirring evenly to obtain the bonding coating.

5. The method for preparing a lightning protection, heat storage and ice protection film suitable for the leading edge of a wind turbine blade according to claim 4, characterized in that: The preparation process of the modified nano boron nitride is as follows: (1) placing a boron nitride raw material in water and stirring at high speed to obtain a boron nitride suspension; (2) adding tris(hydroxymethylaminomethane) to water to obtain a tris(hydroxymethylaminomethane) buffer solution, mixing the tris(hydroxymethylaminomethane) buffer solution and the boron nitride suspension, adding polydopamine, stirring, and then adding NaOH to adjust the pH value of the system to 8.5, and stirring to obtain a mixed solution; (3) After the mixed solution obtained in step (2) is centrifuged several times, the precipitate in the lower layer is collected and freeze-dried each time to obtain polydopamine-coated boron nitride, which is modified nano boron nitride.

6. The method for preparing a lightning protection, heat storage and ice protection film suitable for the leading edge of a wind turbine blade according to claim 1, characterized in that: The preparation process of the bonded heat storage protective film is as follows: Step 1, after mixing the hydrated salt / SiC composite phase change filler and the silane coupling agent KH550, toluene is added to prepare a mixed system; the mixed system is placed in a constant temperature oil bath filtration pot, nitrogen is introduced for stirring, and after the reaction is completed, vacuum filtration is performed, the vacuum filtration product is subjected to ultrasonic treatment and then vacuum filtered again, the filtration product is washed with N,N-dimethylformamide and then dried to obtain a modified hydrated salt / SiC composite phase change filler powder; Step 2, mixing the hydrated salt / SiC composite phase change filler powder and the polyurethane prepolymer, adding the post-chain extender and stirring, and obtaining an insulating, highly thermally conductive, anti-icing dispersion after stirring; Step 3, adding dispersant, titanium dioxide, carbon black, anti-settling agent, defoaming agent, leveling agent, light stabilizer, ultraviolet absorber and solvent to the insulating high thermal conductivity anti-icing dispersion in sequence, stirring and dispersing, and obtaining coating A; Step 3, mixing coating A and water-based isocyanate to obtain a heat storage coating; Step 4, vacuum-infusing the heat storage coating into a film-making mold, and drying it to obtain a heat storage protective film.

7. The method for preparing a lightning protection, heat storage and ice protection film suitable for the leading edge of a wind turbine blade according to claim 1, characterized in that: In step 1, the preparation process of the hydrated salt / SiC composite phase change filler is: (1) mixing dipotassium hydrogen phosphate hexahydrate and disodium hydrogen phosphate dodecahydrate, heating and stirring to obtain a molten eutectic hydrate salt; (2) adding insulating thermal conductive filler silicon carbide to the molten eutectic hydrate salt, and stirring to obtain a eutectic hydrate salt / SiC mixture; (3) adding aluminum dihydrogen phosphate bonding coating to the eutectic hydrate salt / SiC mixture to obtain a mixture; (4) drying the mixture and then sintering it to obtain a sintered product; (5) The sintered product is ball-milled to obtain a hydrated salt / SiC composite phase change filler.

8. The method for preparing a lightning protection, heat storage and ice protection film suitable for the leading edge of a wind turbine blade according to claim 1, characterized in that: In step 2, the preparation process of the polyurethane prepolymer is: The dried polyether diol is placed in a container, nitrogen is introduced into the container, the first catalyst and diisocyanate are added after stirring, the hydrophilic chain extender is added after stirring, and a stirring reaction is carried out, the reaction product is cooled, and a neutralizing agent is added for neutralization reaction to obtain a polyurethane prepolymer.

9. The method for preparing a lightning protection, heat storage and ice protection film suitable for the leading edge of a wind turbine blade according to claim 8, characterized in that: The hydrophilic chain extender is 2,2-dimethylol propionic acid, dimethylol butyric acid or a mixture of the two; The first catalyst is one or more of dibutyltin dilaurate, stannous octoate, and dibutyltin oxide.

10. A lightning protection, heat storage and ice protection film suitable for the leading edge of a wind turbine blade, prepared by the preparation method according to any one of claims 1 to 9, characterized in that: include: Thermal insulation fibers are arranged outside the wind turbine blades; A heat storage protective film is arranged outside the heat insulation fiber; The heat-insulating fibers and the wind turbine blades are bonded together by an adhesive coating, and the heat-storage protective film and the heat-insulating fibers are bonded together by an adhesive coating.

Citation Information

Patent Citations

  • Anti-icing coating and fan blade

    CN116355468A

  • Anti-icing composite coating for wind power blade and preparation method of anti-icing composite coating

    CN116428133A

  • Polyurethane-ceramic composite coating and spraying method

    CN117143512A