Method and system for producing iron ore concentrate and co-producing sulfuric acid by using ferrous sulfate
Through the co-production system of the rotary kiln and sulfuric acid absorption tower, the iron trioxide and sulfur trioxide flue gas generated by ferrous sulfate calcination are converted into high-quality iron concentrate and sulfuric acid, solving the environmental protection and use problems of ferrous sulfate and realizing the Efficient utilization of resources and value.
Patent Information
- Application Number
- CN202411227679.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The calcination process of traditional ferrous sulfate produces a large amount of sulfur trioxide and sulfur dioxide flue gas, which leads to environmental protection problems. At the same time, the use of ferrous sulfate is limited and there is a lack of new consumption channels and high value-added utilization methods.
The co-production system of rotary kiln and sulfuric acid absorption tower is adopted to generate iron trioxide and sulfur trioxide flue gas by calcining ferrous sulfate at high temperature. The sulfuric acid absorption tower is used to convert sulfur trioxide flue gas into sulfuric acid to achieve iron essence of ferrous sulfate. Co-production of ore and sulfuric acid.
It has realized the resource utilization and value utilization of ferrous sulfate, produced high-quality iron concentrate and sulfuric acid, solved the use and environmental protection problems of ferrous sulfate, and has good economic and environmental benefits.
Smart Images

Figure CN118992984A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of chemical metallurgy, and in particular to a system for producing iron ore concentrate and sulfuric acid with ferrous sulfate. Background Art
[0002] Ferrous sulfate, a by-product of titanium dioxide produced by the sulfuric acid process, is currently mainly used in the production of cement chromium-reducing agents, feed additives, polyferrous sulfate, sulfuric acid blending and other traditional applications. The traditional downstream is saturated; a new use is in the production of iron phosphate. Recently, due to the overcapacity of iron phosphate and a significant reduction in demand, there is an urgent need to develop new uses, increase consumption and improve added value.
[0003] Ferrous sulfate is rich in iron and sulfur and is a good resource of iron and sulfur. Currently, only a small amount is calcined to produce iron red. The sulfur resource is simply neutralized with lime, which causes secondary pollution. Although ferrous sulfate can be processed in large quantities and the ferric oxide produced by high-temperature calcination contains 70% iron and is a high-quality iron concentrate, it will produce a large amount of sulfur trioxide and sulfur dioxide flue gas, bringing major environmental problems. Summary of the invention
[0004] The invention provides a method and system for producing iron concentrate and sulfuric acid by using ferrous sulfate, which solves the existing problems.
[0005] In order to achieve the above object, the present invention adopts the following technical scheme: a method for producing iron concentrate and sulfuric acid with ferrous sulfate, the method comprising the following steps:
[0006] A raw material ferrous sulfate (anhydrous) enters the rotary kiln (1), coal powder is burned by the burner to provide heat for the rotary kiln, cold air is exchanged with the iron concentrate discharged from the rotary kiln in the cooler to recover heat, and then enters the burner to assist combustion, and the ferrous sulfate is oxidized and decomposed by heat in the rotary kiln to produce ferric oxide (iron concentrate) and sulfur trioxide flue gas;
[0007] B The sulfur trioxide flue gas enters the sulfuric acid absorption tower (2), and the sulfuric acid enters the sulfuric acid absorption tower (2) through the sulfuric acid absorption circulation pump (3). In the sulfuric acid absorption tower (2), the sulfuric acid absorbs the sulfur trioxide gas to generate sulfuric acid.
[0008] One end of the rotary kiln (1) is connected to a sulfuric acid absorption tower (2). The rotary kiln (1) comprises a kiln body (4), a rotary drum (5), a connecting sleeve (6), a support frame (7), a feed pipe (8), a discharge pipe (9), a valve (10), an air outlet pipe (11) and a scraping mechanism. The air outlet pipe (11) is connected to one end of the sulfuric acid absorption tower (2). The sulfuric acid absorption tower (2) is connected to a sulfuric acid absorption circulation pump (3) via a circulation pipe.
[0009] The raw material of step A is anhydrous ferrous sulfate, and the rotary kiln operating conditions are: decomposition temperature 900-950° C., reaction time 1 hour, decomposition reaction atmosphere is oxidizing atmosphere, and oxygen content of kiln outlet gas is ≥2-4%.
[0010] The concentration of sulfuric acid in step B is 95-98%, and the control process conditions of the sulfuric acid absorption tower are: temperature 60° C.-80° C., and gas-liquid ratio 500:1.
[0011] High temperature calcination mechanism: The ferrous sulfate heptahydrate is treated by a two-step process of drying and calcination. The drying temperature is controlled at 300-350°C to dehydrate the ferrous sulfate heptahydrate to obtain monohydrate and anhydrous ferrous sulfate. The monohydrate and anhydrous ferrous sulfate enter the rotary kiln for high temperature calcination at a controlled temperature of 900-950°C for 60 minutes with an excess of 10% air. The reactions involved are:
[0012] FeSO4·7H20→FeSO4·H20+6H2O
[0013] FeSO4·7H20→FeSO4+7H20
[0014] 2FeSO4·H20+0.5O2→Fe2O3+2SO3+2H20
[0015] 2FeSO4+0.5O2→Fe2O3+2SO3
[0016] Sulfuric acid absorption mechanism: Sulfuric acid is produced by absorbing sulfur trioxide with sulfuric acid, and the absorption temperature and concentration are controlled by heat exchange to produce qualified sulfuric acid products. The main reactions involved are:
[0017] SO3+H2O→H2SO4
[0018] Preferably, rotating drums are symmetrically arranged at both ends of the kiln body, the kiln body is rotatably connected to the rotating drum, a connecting sleeve is provided on the surface of the rotating drum, the connecting sleeve is connected to the supporting frame, a feed pipe is provided on one end of the rotating drum, a discharge pipe is provided on the other end of the rotating drum, a valve is provided on the discharge pipe, and an air outlet pipe is provided on the other end of the rotating drum.
[0019] Preferably, the scraper mechanism includes a first motor, a scraper ring, a threaded rod, a driving bevel gear, a driven bevel gear, a sliding rod and a protective pad. A threaded rod is provided on one side of the rotary kiln, one end of the threaded rod is connected to the driven bevel gear, a support plate is provided on one side of the rotating drum, a first motor is provided on the support plate, a driving bevel gear is provided on the output shaft of the first motor, the driving bevel gear and the driven bevel gear are meshed with each other, a scraper ring is provided on the threaded rod, a protective pad is provided on the outer side of the scraper ring, and a sliding rod is provided on the other side of the rotary kiln.
[0020] Preferably, a second motor is provided on the surface of the sulfuric acid absorption tower, the output shaft of the second motor is connected to a rotating shaft, one end of the rotating shaft extends into the sulfuric acid absorption tower, and a plurality of stirring shafts are provided on the rotating shaft.
[0021] Preferably, a driven gear is provided on the surface of the kiln body, a support block is provided under the kiln body, a driving motor is provided on the support block, a driving gear is provided on the output shaft of the driving motor, and the driven gear meshes with the driving gear.
[0022] Preferably, the air inlet of the sulfuric acid absorption tower is connected to the air outlet pipe, a gas outlet is provided on one side of the sulfuric acid absorption tower, and a discharge port is provided below the gas outlet.
[0023] Preferably, the rotary kiln is connected to one end of the burner, and the other end of the burner is connected to a cooler.
[0024] Preferably, the other end of the rotary kiln is connected to a cooler.
[0025] A system for producing iron concentrate from ferrous sulfate and co-producing sulfuric acid is characterized by being formed by structural connection as used in the above method.
[0026] The beneficial effects of the present invention are as follows: the method is combined with the system, the high-temperature decomposition atmosphere of ferrous sulfate is changed into an oxidizing atmosphere, the flue gas generated is sulfur trioxide, and sulfuric acid is used to absorb the sulfur trioxide to produce a sulfuric acid product, while at the same time, the ferric oxide (containing about 70% iron) produced by calcining ferrous sulfate is a high-quality iron concentrate, and the generated sulfur trioxide gas is absorbed by sulfuric acid to produce a sulfuric acid product, so that the production of iron concentrate and the co-production of sulfuric acid by ferrous sulfate are achieved, and the iron resources in the low-value ferrous sulfate produced as a by-product of titanium dioxide in the sulfuric acid process are used to produce high-quality iron concentrate, and the sulfur resources are used to produce sulfuric acid, so that the by-product ferrous sulfate can be utilized as a resource and value, and the problem of the outlet of the ferrous sulfate produced as a by-product of titanium dioxide in the sulfuric acid process is completely solved, with good economic and environmental benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The figure is a system flow chart of the method of the present invention.
[0028] Figure 2 It is a schematic diagram of the connection structure of the rotary kiln and the sulfuric acid absorption tower of the present invention.
[0029] Figure 3 It is a schematic diagram of the cross-sectional structure of the rotary kiln of the present invention.
[0030] Figure 4 It is a schematic diagram of the cross-sectional structure of the sulfuric acid absorption tower of the present invention.
[0031] Numbers in the figure: 1. rotary kiln; 2. sulfuric acid absorption tower; 3. sulfuric acid absorption circulation pump; 4. kiln body; 5. rotating drum; 6. connecting sleeve; 7. supporting frame; 8. feeding pipe; 9. discharging pipe; 10. valve; 11. air outlet pipe; 12. first motor; 13. scraper ring; 14. threaded rod; 15. driving bevel gear; 16. driven bevel gear; 17. sliding rod; 18. protective pad; 19. second motor; 20. rotating shaft; 21. stirring shaft; 22. driven gear; 23. supporting block; 24. driving motor; 25. driving gear; 26. air inlet; 27. air outlet; 28. discharging port. DETAILED DESCRIPTION
[0032] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0033] Embodiment 1
[0034] Reference Figure 1-Figure 4 As shown, a method for producing iron concentrate and sulfuric acid with ferrous sulfate comprises the following steps:
[0035] A raw material ferrous sulfate (anhydrous) enters the rotary kiln (1), coal powder is burned by the burner to provide heat for the rotary kiln, cold air is exchanged with the iron concentrate discharged from the rotary kiln in the cooler to recover heat, and then enters the burner to assist combustion, and the ferrous sulfate is oxidized and decomposed by heat in the rotary kiln to produce ferric oxide (iron concentrate) and sulfur trioxide flue gas;
[0036] B The sulfur trioxide flue gas enters the sulfuric acid absorption tower (2), and the sulfuric acid enters the sulfuric acid absorption tower (2) through the sulfuric acid absorption circulation pump (3). In the sulfuric acid absorption tower (2), the sulfuric acid absorbs the sulfur trioxide gas to generate sulfuric acid.
[0037] One end of the rotary kiln (1) is connected to a sulfuric acid absorption tower (2). The rotary kiln (1) comprises a kiln body (4), a rotary drum (5), a connecting sleeve (6), a support frame (7), a feed pipe (8), a discharge pipe (9), a valve (10), an air outlet pipe (11) and a scraping mechanism. The air outlet pipe (11) is connected to one end of the sulfuric acid absorption tower (2). The sulfuric acid absorption tower (2) is connected to a sulfuric acid absorption circulation pump (3) via a circulation pipe.
[0038] The raw material of step A is anhydrous ferrous sulfate, and the rotary kiln operating conditions are: decomposition temperature 900-950° C., reaction time 1 hour, decomposition reaction atmosphere is oxidizing atmosphere, and oxygen content of kiln outlet gas is ≥2-4%.
[0039] The concentration of sulfuric acid in step B is 95-98%, and the control process conditions of the sulfuric acid absorption tower are: temperature 60° C.-80° C., and gas-liquid ratio 500:1.
[0040] High temperature calcination mechanism: The ferrous sulfate heptahydrate is treated by a two-step process of drying and calcination. The drying temperature is controlled at 300-350°C to dehydrate the ferrous sulfate heptahydrate to obtain monohydrate and anhydrous ferrous sulfate. The monohydrate and anhydrous ferrous sulfate enter the rotary kiln for high temperature calcination at a controlled temperature of 900-950°C for 60 minutes with an excess of 10% air. The reactions involved are:
[0041] FeSO4·7H20→FeSO4·H20+6H2O
[0042] FeSO4·7H20→FeSO4+7H20
[0043] 2FeSO4·H20+0.5O2→Fe2O3+2SO3+2H20
[0044] 2FeSO4+0.5O2→Fe2O3+2SO3
[0045] Sulfuric acid absorption mechanism: Sulfuric acid is produced by absorbing sulfur trioxide with sulfuric acid, and the absorption temperature and concentration are controlled by heat exchange to produce qualified sulfuric acid products. The main reactions involved are:
[0046] SO3+H2O→H2SO4
[0047] Rotating drums 5 are symmetrically arranged at both ends of the kiln body 4, and the kiln body 4 is rotatably connected to the rotating drum 5. A connecting sleeve 6 is arranged on the surface of the rotating drum 5, and the connecting sleeve 6 is connected to the supporting frame 7. A feeding pipe 8 is arranged on one end of the rotating drum 5, and a discharging pipe 9 is arranged on the other end of the rotating drum 5. A valve 10 is arranged on the discharging pipe 9, and an air outlet pipe 11 is arranged on the other end of the rotating drum 5. The scraping mechanism includes a first motor 12, a scraping ring 13, a threaded rod 14, an active bevel gear 15, a driven bevel gear 16, a sliding rod 17 and a protective pad 18. A threaded rod 14 is arranged on one side of the rotary kiln 1, and one end of the threaded rod 14 is connected to the driven bevel gear 16. One side of the rotating drum 5 A support plate is provided, and a first motor 12 is provided on the support plate. A driving bevel gear 15 is provided on the output shaft of the first motor 12. The driving bevel gear 15 and the driven bevel gear 16 are meshed with each other. A scraper ring 13 is provided on the threaded rod 14. A protective pad 18 is provided on the outer side of the scraper ring 13. A sliding rod 17 is provided on the other side of the rotary kiln 1. When the first motor 12 works, the driving bevel gear 15 rotates, driving the driven bevel gear 16 to rotate, so that the threaded rod 14 rotates, so that the scraper ring 13 moves on the threaded rod 14, and the material remaining on the inner wall is scraped off, so that it is convenient to clean it and ensure the cleanliness of the inner wall.
[0048] A second motor 19 is provided on the surface of the sulfuric acid absorption tower 2, and the output shaft of the second motor 19 is connected to a rotating shaft 20. One end of the rotating shaft 20 extends into the sulfuric acid absorption tower 2. A plurality of stirring shafts 21 are provided on the rotating shaft 20. When the second motor 19 works, the stirring shafts 21 on the rotating shaft 20 are driven to rotate, thereby accelerating the mixed absorption. A driven gear 22 is provided on the surface of the kiln body 4, and a support block 23 is provided under the kiln body 4. A driving motor 24 is provided on the support block 23. A driving gear 25 is provided on the output shaft of the driving motor 24. The driven gear 22 and the driving gear 25 are meshed with each other. When the driving motor 24 works, the driving gear 25 is driven to rotate, thereby driving the driven gear 22 and the kiln body 4 to rotate, thereby accelerating the thermal oxidation decomposition.
[0049] The air inlet 26 of the sulfuric acid absorption tower 2 is connected to the air outlet pipe 11, an air outlet 27 is provided on one side of the sulfuric acid absorption tower 2, and a discharge port 28 is provided below the air outlet 27. The rotary kiln 1 is connected to one end of the burner, and the other end of the burner is connected to the cooler. The other end of the rotary kiln 1 is connected to the cooler. The cold air enters the burner to assist combustion after the cooler and the rotary kiln 1 discharge the iron concentrate for heat exchange and heat recovery.
[0050] The system of the above-mentioned method of use is also a system for producing iron concentrate and sulfuric acid by ferrous sulfate, and its working principle is as follows: the raw material ferrous sulfate enters the rotary kiln 1, and the coal powder is burned by the burner to provide heat for the rotary kiln 1. The cold air exchanges heat with the iron concentrate discharged from the rotary kiln 1 in the cooler and recovers heat before entering the burner to assist combustion. In the rotary kiln 1, the ferrous sulfate is oxidized and decomposed by heat to produce ferric oxide and sulfur trioxide flue gas. The ferric oxide is the iron concentrate, and the sulfur trioxide flue gas enters the sulfuric acid absorption tower 2. The sulfuric acid enters the sulfuric acid absorption tower 2 through the sulfuric acid absorption circulation pump 3. In the sulfuric acid absorption tower 2, the sulfuric acid absorbs the sulfur trioxide gas to generate sulfuric acid, and the sulfuric acid product is transported out of the system through the sulfuric acid absorption circulation pump 3.
[0051] The production of iron concentrate and sulfuric acid from ferrous sulfate is realized. The iron resources in the low-value ferrous sulfate produced as a by-product of titanium dioxide produced by the sulfuric acid process are used to produce high-quality iron concentrate, and the sulfur resources are used to produce sulfuric acid. Ultimately, the by-product ferrous sulfate can be utilized as a resource and value, which completely solves the problem of the outlet of ferrous sulfate produced as a by-product of titanium dioxide produced by the sulfuric acid process, and has good economic and environmental benefits.
[0052] Embodiment 2
[0053] The combination of the process flow and system structure of the first embodiment is still adopted, and the requirements different from those of the first embodiment are:
[0054] Control ferrous sulfate at 100kg / h, rotary kiln calcination temperature at 930℃, calcination time at 1 hour, and oxygen content in flue gas at 3%;
[0055] Sulfuric acid absorption tower control: absorption liquid sulfuric acid concentration 98%, temperature 60°C, gas-liquid ratio 500:1.
[0056] According to the above process, the results are analyzed and obtained as follows:
[0057] Iron concentrate: iron content 68.1%
[0058] Sulfuric acid: H2SO4 98.1%.
[0059] Embodiment 3
[0060] The combination of the process flow and system structure of the first embodiment is still adopted, and the requirements different from those of the first embodiment are:
[0061] Control the ferrous sulfate to 100kg / h, the calcination temperature to 950℃, the calcination time to 1 hour, and the oxygen content in the flue gas to 4%;
[0062] Sulfuric acid absorption tower control: absorption liquid sulfuric acid concentration 98%, temperature 65°C, gas-liquid ratio 500:1.
[0063] According to the above process, the results are analyzed and obtained as follows:
[0064] Iron concentrate: iron content 67.8%
[0065] Sulfuric acid: H2SO4 98.2%.
[0066] Embodiment 4
[0067] The combination of the process flow and system structure of the first embodiment is still adopted, and the requirements different from those of the first embodiment are:
[0068] Control the ferrous sulfate to 200kg / h, the calcination temperature to 940℃, the calcination time to 1 hour, and the oxygen content in the flue gas to 2%;
[0069] Sulfuric acid absorption tower control: absorption liquid sulfuric acid concentration 98%, temperature 60°C, gas-liquid ratio 500:1.
[0070] According to the above process, the results are analyzed and obtained as follows:
[0071] Iron concentrate: iron content 66.9%
[0072] Sulfuric acid: H2SO4 98.5%.
[0073] From the above, it can be concluded that: ferrous sulfate produces iron concentrate and sulfuric acid, and the produced ferric oxide (containing about 70% iron) is high-quality iron concentrate.
[0074] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for producing iron concentrate and sulfuric acid from ferrous sulfate, characterized in that: The method comprises the following steps: A raw material ferrous sulfate (anhydrous) enters a rotary kiln (1); pulverized coal is burned by a burner to provide heat for the rotary kiln; cold air exchanges heat with the iron concentrate discharged from the rotary kiln in a cooler to recover heat and then enters a burner to assist combustion; the ferrous sulfate is oxidized and decomposed by heat in the rotary kiln to produce ferric oxide (iron concentrate) and sulfur trioxide flue gas; B the sulfur trioxide flue gas enters a sulfuric acid absorption tower (2); sulfuric acid enters the sulfuric acid absorption tower (2) through a sulfuric acid absorption circulation pump (3); sulfuric acid absorbs sulfur trioxide gas in the sulfuric acid absorption tower (2) to generate sulfuric acid.
2. The method for producing iron concentrate and sulfuric acid from ferrous sulfate according to claim 1, characterized in that: One end of the rotary kiln (1) is connected to a sulfuric acid absorption tower (2). The rotary kiln (1) comprises a kiln body (4), a rotary drum (5), a connecting sleeve (6), a support frame (7), a feed pipe (8), a discharge pipe (9), a valve (10), an air outlet pipe (11) and a scraping mechanism. The air outlet pipe (11) is connected to one end of the sulfuric acid absorption tower (2). The sulfuric acid absorption tower (2) is connected to a sulfuric acid absorption circulation pump (3) via a circulation pipe.
3. The method for producing iron ore concentrate and sulfuric acid by using ferrous sulfate according to claim 1, characterized in that: The raw material of step A is anhydrous ferrous sulfate, and the rotary kiln operating conditions are: decomposition temperature 900-950° C., reaction time 1 hour, decomposition reaction atmosphere is oxidizing atmosphere, and oxygen content of kiln outlet gas is ≥2-4%.
4. The method for producing iron ore concentrate and sulfuric acid by using ferrous sulfate according to claim 1, characterized in that: The concentration of sulfuric acid in step B is 95-98%, and the control process conditions of the sulfuric acid absorption tower are: temperature 60° C.-80° C., and gas-liquid ratio 500:
1.
5. The method for producing iron ore concentrate and sulfuric acid by using ferrous sulfate according to claim 2, characterized in that: Rotating drums (5) are symmetrically arranged at both ends of the kiln body (4), the kiln body (4) is rotatably connected to the rotating drum (5), a connecting sleeve (6) is provided on the surface of the rotating drum (5), the connecting sleeve (6) is connected to the support frame (7), a feeding pipe (8) is provided on one end of the rotating drum (5), a discharging pipe (9) is provided on the other end of the rotating drum (5), a valve (10) is provided on the discharging pipe (9), an air outlet pipe (11) is provided on the other end of the rotating drum (5), the rotary kiln (1) is connected to one end of the burner, and the other end of the burner is connected to a cooler.
6. The method for producing iron ore concentrate and sulfuric acid by using ferrous sulfate according to claim 2, characterized in that: The scraping mechanism comprises a first motor (12), a scraping ring (13), a threaded rod (14), a driving bevel gear (15), a driven bevel gear (16), a sliding rod (17) and a protection pad (18). A threaded rod (14) is provided on one side of the rotary kiln (1), one end of the threaded rod (14) is connected to the driven bevel gear (16), a support plate is provided on one side of the rotating drum (5), a first motor (12) is provided on the support plate, a driving bevel gear (15) is provided on the output shaft of the first motor (12), the driving bevel gear (15) and the driven bevel gear (16) are meshed with each other, a scraping ring (13) is provided on the threaded rod (14), a protection pad (18) is provided on the outer side of the scraping ring (13), and a sliding rod (17) is provided on the other side of the rotary kiln (1).
7. The method for producing iron ore concentrate and sulfuric acid by using ferrous sulfate according to claim 2, characterized in that: A second motor (19) is provided on the surface of the sulfuric acid absorption tower (2); an output shaft of the second motor (19) is connected to a rotating shaft (20); one end of the rotating shaft (20) extends into the sulfuric acid absorption tower (2); a plurality of stirring shafts (21) are provided on the rotating shaft (20); an air inlet (26) of the sulfuric acid absorption tower (2) is connected to an air outlet pipe (11); an air outlet (27) is provided on one side of the sulfuric acid absorption tower (2); and a material outlet (28) is provided below the air outlet (27).
8. The method for producing iron ore concentrate and sulfuric acid by using ferrous sulfate according to claim 6, characterized in that: A driven gear (22) is provided on the surface of the kiln body (4), a support block (23) is provided below the kiln body (4), a driving motor (24) is provided on the support block (23), a driving gear (25) is provided on the output shaft of the driving motor (24), and the driven gear (22) and the driving gear (25) are meshed with each other.
9. A system for producing iron concentrate and sulfuric acid by ferrous sulfate, characterized in that: A structural connection formed by using the method according to any one of claims 1 to 8.
Citation Information
Patent Citations
Method for preparing iron oxide red and sulfuric acid by sulfate capable of decomposing iron by sulfur reduction
CN103553143A
Desulfurization tower for sulfuric acid tail gas
CN107281923A
Rotary kiln reactor with multiple layers of barrels
CN116878268A
High-temperature aluminum oxide calcining kiln
CN117781671A
Method and system for producing iron ore concentrate and co-producing phosphoric acid based on ferrous sulfate
CN118324195A