Method for preparing phosphorene nanobelt through mechanical stripping
Through mechanical peeling and PDMS contact peeling methods, the defects of high-energy electron beam and liquid-phase peeling methods in the prior art were solved, and high-quality, smooth edges and different orientations were successfully prepared, achieving low cost and high efficiency production.
Patent Information
- Application Number
- CN202411118260.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-22
AI Technical Summary
In the prior art, high-energy electron beams are expensive to prepare phosphorene nanoribbons, low yield, and many edge defects. The liquid phase peeling method is easy to contaminate the product, making it difficult to prepare high-quality one-dimensional black phosphorene nanoribbons.
The phosphorene nanoribbons were prepared by the contact stripping method of tape and PDMS by mechanical peeling method. Multiple mechanical peeling and dry transfer techniques were used to obtain high-quality, smooth edges and different orientations of phosphorene nanoribbons.
It realizes the preparation of high-quality phosphorene nanoribbons at low cost and high efficiency, avoids chemical reactions and the use of harmful substances, and is characterized by green and environmental protection and easy to produce on a large scale.
Smart Images

Figure CN118992994A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of semiconductor material preparation, and in particular to a method for preparing phosphorene nanoribbons by mechanical exfoliation. Background Art
[0002] Black phosphorus (BP) is a single element substance of phosphorus and an allotrope of white phosphorus and red phosphorus. Black phosphorus was successfully prepared as early as 1914, but it did not attract much attention. It was not until 2014 that black phosphorus re-entered people's field of vision and received high attention based on the successful preparation of few-layer black phosphorus field-effect transistors and the excellent electrical properties they exhibited. Black phosphorus is a p-type direct bandgap semiconductor material whose bandgap can be regulated by changing the number of layers, ranging from about 0.3 eV in bulk to about 2 eV in a single layer. The room temperature hole mobility and current switching ratio of two-dimensional black phosphorus (2D BP) can be as high as 1000 cm 2 V -l s -1 and 10 5 In addition, black phosphorus has the characteristics of in-plane anisotropy and non-toxicity, showing great application potential in high-performance optoelectronic devices, photocatalysis, thermoelectric materials and biomedical materials.
[0003] Compared with two-dimensional black phosphorus, one-dimensional phosphorene nanoribbons inherit all the excellent properties of two-dimensional black phosphorus or phosphorene in electronics and optoelectronics, and due to the special edge confinement effect of one-dimensional phosphorene nanoribbons, they have more flexible band gap adjustable properties and greater practical value in the semiconductor neighborhood than two-dimensional black phosphorus or phosphorene. For example, in terms of conductivity, due to the anisotropy of black phosphorus, the orientation of one-dimensional phosphorene nanoribbons can affect the effectiveness of its interlayer and intralayer electron transmission. Nanoribbons with good orientation are more likely to form continuous intralayer conductive channels, thereby providing better conductivity performance. In terms of band gap regulation, the band gap of black phosphorus can be regulated by the number of layers and orientation. In one-dimensional phosphorene nanoribbons, changes in orientation can lead to changes in the band gap, which in turn affects its optical and electrical properties. Therefore, the preparation of one-dimensional phosphorene nanoribbons with different boundary orientations can achieve precise regulation of the band gap, providing more possibilities for the design of optoelectronic devices and nanoelectronic devices.
[0004] However, there are few studies on the preparation of one-dimensional phosphorene nanoribbons, which can be mainly divided into two categories: the first category is to use high-energy electron beams to cut large areas of black phosphorus into nanoribbons, such as journal literature (Nat Commun 2015, 6, 8573) and (ACS Nano 2016, 10, 5687-5695). The shortcomings of this type of preparation method are that it requires expensive equipment, low yield, limited processing accuracy, and the edge structure of the prepared BPNR or PNR is messy. At the same time, due to exposure to high-energy particles, there are some defects in the nanoribbon structure, which will affect the intrinsic properties of the nanoribbon. The second category is to prepare one-dimensional phosphorene nanoribbons by liquid phase exfoliation method using intercalation or non-intercalation method. After searching the prior art, it was found that Chinese patent document number CN104961113A, published (announced) date 2015.10.07, discloses a method for preparing phosphorene, including: dispersing black phosphorus in a dispersion, and ultrasonically treating it for 0.5 to 200 hours, and then performing solid-liquid separation to obtain intercalated black phosphorus; dispersing the intercalated black phosphorus in a chemical foaming agent solution, and ultrasonically treating it for 0.5 to 200 hours, and then performing solid-liquid separation, and then drying the solid after solid-liquid separation to obtain a solid mixture of black phosphorus and the chemical foaming agent; subjecting the solid mixture of black phosphorus and the chemical foaming agent to microwave treatment, the microwave power is 100 to 1000W, and after microwave treatment for 1 second to 1 hour, the finished phosphorene is obtained. However, the yield of single-layer phosphorene in the preparation of phosphorene by the prior art is not high, the size and appearance of the prepared phosphorene are uncontrollable, and phosphorene with a one-dimensional strip-shaped morphology cannot be prepared. Patent CN105668531A discloses a liquid phase exfoliation method for preparing phosphorene nanoribbons or phosphorus nanoribbons, wherein strip-shaped or flaky black phosphorus is mixed with an organic solvent, and then subjected to ultrasonic transverse tearing treatment and centrifugal treatment in sequence, and the supernatant rich in phosphorene nanoribbons in the product is dripped onto a substrate and then obtained by spin coating or drying. The prepared phosphorene nanoribbons have better quality, low method cost, high yield, and are conducive to further scientific research and promotion and application of phosphorene nanoribbons. Although the liquid phase exfoliation method has the advantages of simplicity and scalable production, the liquid in the preparation process is prone to contamination of the product. Therefore, the preparation of high-quality one-dimensional black phosphorene nanoribbons is still facing great challenges. Summary of the invention
[0005] The present invention aims to solve the shortcomings of the prior art in which phosphorene nanoribbons (PNR) prepared by high-energy electron beams are high in cost, low in yield, many in edge defects, unstable in quality, and the prepared phosphorene nanoribbons are easily contaminated during the preparation process by liquid phase exfoliation. The present invention provides a method for preparing phosphorene nanoribbons by mechanical exfoliation. The method has low cost and high quality, and is conducive to further scientific research and popularization and application of phosphorene nanoribbons.
[0006] To achieve the above object, the present invention provides the following solutions:
[0007] One of the technical solutions of the present invention is to provide a method for preparing phosphorene nanoribbons by mechanical exfoliation, the steps comprising:
[0008] S1, the black phosphorus polycrystalline sample was peeled off multiple times by mechanical stripping tape to obtain a thick BP sheet with partially peeled PNRs on the tape;
[0009] S2. The partially peeled PNRs are further peeled off by the tape-PDMS contact peeling method to obtain separated and independent PNRs on PDMS.
[0010] S3, transferring the PNRs on the PDMS to the substrate by a conventional dry transfer method to obtain a substrate with PNRs fixed thereon;
[0011] S4. Soaking the substrate with the PNRs fixed thereon in an organic solvent and then drying it to obtain phosphorene nanoribbons.
[0012] Furthermore, the black phosphorus polycrystalline sample is a crystal with multiple boundary characteristics.
[0013] The purpose of using crystals with multiple boundary features is to obtain PNRs with different lattice orientations along the length direction.
[0014] Furthermore, the multiple peelings are performed 3 to 5 times.
[0015] When the number of stripping times is less than 3 times, the too low stripping frequency will only produce a small amount of partially stripped PNRs. When the number of stripping times exceeds 5 times, the excessive stripping frequency will result in only small BP fragments or two-dimensional BP sheets that are peeled off from large BP crystals.
[0016] During multiple stripping operations, the tape with the stripped product attached is placed on the nearest adjacent, new, clean area each time to avoid overlapping of the PNRs finally produced.
[0017] Furthermore, the steps of the tape-PDMS contact stripping method are:
[0018] The tape carrying the thick BP sheet with partially peeled PNRs was pressed onto the PDMS surface, and then the tape was torn off to achieve further peeling, thereby obtaining separated, independent PNRs on the PDMS.
[0019] Furthermore, in step S2, the thickness of the PNRs of the PDMS is 1 nm to 100 nm, the width is 15 nm to 1 μm, and the length is 1 μm to 70 μm.
[0020] Furthermore, the dry transfer step is: pressing the PDMS with separated and independent PNRs onto a substrate and keeping it at 40-65° C. for 5-10 minutes, and then separating the PDMS and the substrate; the substrate is a rigid substrate or a flexible substrate.
[0021] Preferably, the rigid substrate includes one of a Si substrate, a SiO2 / Si substrate, a ceramic substrate and an ITO conductive glass.
[0022] Preferably, the flexible substrate comprises a polyamide (PI) resin film or a polyethylene terephthalate (PET) resin film.
[0023] Furthermore, the organic solvent includes at least one of an alcohol organic solvent, an ether organic solvent, a ketone organic solvent, a benzene ring organic solvent, dimethyl sulfoxide and dimethylformamide.
[0024] Preferably, the alcohol organic solvent includes at least one of methanol, ethanol and isopropanol.
[0025] Preferably, the ether organic solvent includes diethyl ether and / or phenethyl ether.
[0026] Preferably, the ketone organic solvent includes acetone and / or N-methylpyrrolidone.
[0027] Preferably, the benzene ring organic solvent includes at least one of benzene, toluene and phenol.
[0028] The purpose of organic solvent soaking and oxygen plasma treatment is to remove the residues of mechanical release tape and thermal release adhesive.
[0029] Furthermore, the drying includes one of inert gas air drying, freeze drying and vacuum oven drying.
[0030] Preferably, the inert gas includes N2 and / or Ar gas.
[0031] The second technical solution of the present invention is to provide a phosphorene nanoribbon prepared by the above method.
[0032] Furthermore, the black phosphorus nanoribbon or phosphorene nanoribbon has a thickness of 1 nm to 100 nm, a width of 15 nm to 1 μm, a length of 1 μm to 70 μm, and has different lattice orientations in the length direction.
[0033] According to the specifications of black phosphorus polycrystalline samples, the length of phosphorene nanoribbons is between 1μm and 70μm.
[0034] The third technical solution of the present invention is to provide an application of the above-mentioned black phosphorus nanoribbon or phosphorene nanoribbon in electronic and optoelectronic devices or sensor devices.
[0035] Furthermore, the electronic and optoelectronic devices or sensor devices include field effect transistors, diodes, solar photovoltaic cells, photoelectric detection devices, gas sensors or memristors.
[0036] The present invention discloses the following technical effects:
[0037] The present invention proposes a novel mechanical exfoliation method, which uses a two-step exfoliation method combining tape exfoliation and polydimethylsiloxane (PDMS) exfoliation to prepare high-quality, narrow, differently oriented, and smooth-edged PNRs for the first time. Partially exfoliated PNRs are first formed on a relatively thick BP sheet by tape exfoliation, and then further exfoliated by the direct interaction force between PDMS and the tape to obtain separated single PNRs. The width of the prepared PNRs ranges from a dozen nanometers to 1μm, the smallest to 15nm, and the average length is 18μm. At the same time, the prepared PNRs have different boundary orientations.
[0038] The phosphorene nanoribbons prepared by the present invention are of high quality, no chemical reaction is involved in the preparation process, and no toxic or harmful substances are added. The invention has the characteristics of being green and environmentally friendly, low cost, simple process, high production efficiency, and easy to scale up, which is conducive to further scientific research and popularization and application of phosphorene nanoribbons. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0040] Figure 1 Schematic diagram of the preparation process of the present invention, wherein (a) is mechanical stripping of tape, (b) is contact stripping of tape-PDMS, and (c) is transfer to substrate;
[0041] Figure 2 The thick BP sheet of partially peeled PNRs carried by the tape of Example 1;
[0042] Figure 3 This is an optical microscope photo of the PNRs peeled off in Example 1;
[0043] Figure 4 This is an optical microscope image of A during angle-resolved polarization Raman testing;
[0044] Figure 5 is the Raman spectrum of A at different polarization angles of 30° to 210° with an interval of 30°;
[0045] Figure 6 The Raman spectrum of A is normalized using Coordinate graphs plotting band intensities;
[0046] Figure 7 : is the angle-resolved polarization Raman spectrum of B, wherein (a) is the result of the angle-resolved polarization Raman characteristic of B, and (b) is the polar coordinate diagram of B;
[0047] Figure 8 is a polarization Raman spectrum of C, wherein (a) is the result of the angle-resolved polarization Raman characteristic of C, and (b) is the polar coordinate diagram of C;
[0048] Fig. 9 This is a scanning electron microscope photograph of the phosphorene nanoribbon prepared in Example 2;
[0049] Fig.10 This is a scanning electron microscope photograph of the phosphorene nanoribbon prepared in Comparative Example 1. DETAILED DESCRIPTION
[0050] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0051] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0052] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0053] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0054] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0055] Figure 1 Schematic diagram of the preparation process of the present invention, wherein (a) is mechanical stripping of the tape, (b) is contact stripping of the tape-PDMS, and (c) is transfer to a substrate.
[0056] Example 1
[0057] The method steps for preparing phosphorene nanoribbons by mechanical exfoliation are as follows:
[0058] S1. The black phosphorus polycrystalline sample with multi-boundary features was placed on a mechanical exfoliation tape and exfoliated three times. Each time, the tape with the exfoliated product attached was placed on the nearest, new, clean area for exfoliation, and a thick BP sheet with partially exfoliated PNRs was obtained on the tape.
[0059] S2, pressing a tape with a thick BP sheet carrying partially peeled PNRs onto a polydimethylsiloxane (PDMS) surface, and then removing the tape to obtain single, independent PNRs on the PDMS;
[0060] S3. Using a dry transfer method, the PDMS with PNRs was pressed onto a target substrate (300 nm, SiO2 / Si), and the press was performed at 50°C for 5 min to separate the PDMS from the surface of the target substrate to obtain a substrate with PNRs fixed thereon;
[0061] S4. Soak the substrate with PNRs fixed in acetone for 24 hours to remove the residues of the mechanical stripping tape and PDMS, then take out the sample and blow dry it with nitrogen to obtain the PNRs sample.
[0062] Figure 2 The thick BP sheet of partially peeled PNRs with the tape of Example 1 is composed of Figure 2 It can be seen that among the partially peeled PNRs, some have one end lifted up and the other end connected to the BP sheet, some PP bonds between PNRs and BP sheets are all broken, and embossed structures appear on the BP sheet, while others are embedded in the BP sheet, with only the PP bonds at the edges broken.
[0063] Figure 3 This is an optical microscope photograph of the PNRs peeled off in Example 1.
[0064] Three PNRs were selected for polarization Raman spectroscopy testing, named A, B and C, to determine the crystal orientation of PNRs along the length direction. The polarization Raman spectrum of A is shown in Figures 4 to 6, and the polarization Raman spectrum of B is shown in Figure Figure 7 As shown, the polarization Raman spectrum of C is as follows Figure 8 shown.
[0065] Figure 4 This is an optical microscope image of A during angle-resolved polarization Raman testing; Figure 5 is the Raman spectrum of A at different polarization angles of 30° to 210° with an interval of 30°; Figure 6 The Raman spectrum of A is normalized using The intensity of the band is plotted in a coordinate graph. Figures 4 to 6 It can be seen that The intensity of the band changes with the polarization angle in a period of 180°. When the Raman laser polarization direction is along the Armchair direction and Zigzag direction of the BP crystal, The band strengths are the strongest and weakest, respectively, such as Figure 6 As shown by the arrow in the middle. Figure 4 The length direction of A measured in Figure 6 From the correlation of the direction of the arrow in the figure, we can judge that the length direction of A is along the Zigzag direction.
[0066] Figure 7 : is the angle-resolved polarization Raman spectrum of B, wherein (a) is the result of the angle-resolved polarization Raman characteristic of B, and (b) is the polar coordinate diagram of B; Figure 8 The polarization Raman spectrum of C, where (a) is the result of the angle-resolved polarization Raman characteristics of C, and (b) is the polar coordinate diagram of C. Figures 7-8 It can be seen that the length directions of B and C are the Armchair and the direction at 30° to the Armchair, respectively, which further proves that the prepared BPNR or PNR has different boundary orientations.
[0067] Example 2
[0068] The method steps for preparing phosphorene nanoribbons by mechanical exfoliation are as follows:
[0069] S1. The black phosphorus polycrystalline sample with multi-boundary features was placed on a mechanical exfoliation tape and exfoliated five times. Each time, the tape with the exfoliated product attached was placed on the nearest, new, clean area for exfoliation, and a thick BP sheet with partially exfoliated PNRs was obtained on the tape.
[0070] S2, pressing the tape carrying the BP sheet with partially peeled PNRs onto the surface of polydimethylsiloxane (PDMS), and then tearing off the tape to obtain single, independent PNRs on the PDMS;
[0071] S3. Using a dry transfer method, press the PDMS with PNRs onto the target substrate (300 nm, SiO2 / Si) at 60°C for 7 min. Separate the PDMS from the surface of the target substrate to obtain a substrate with PNRs fixed thereon;
[0072] S4. Soak the substrate with PNRs fixed in acetone for 24 hours to remove the residues of tape and PDMS, then take out the sample and blow dry it with nitrogen to obtain the PNRs sample.
[0073] Fig. 9 This is a scanning electron microscope photograph of the phosphorene nanoribbon prepared in Example 2.
[0074] Comparative Example 1
[0075] Compared with Example 1, the only difference is that the peeling is performed 10 times in step S1.
[0076] Fig.10 This is a scanning electron microscope photo of the phosphorene nanoribbon prepared in Comparative Example 1. Fig.10 It can be seen that due to too many stripping times, most of the products produced are small BP fragments.
[0077] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for preparing phosphorene nanoribbons by mechanical exfoliation, characterized in that the steps include: S1, the black phosphorus polycrystalline sample was peeled off multiple times by mechanical stripping tape to obtain a thick BP sheet with partially peeled PNRs on the tape; S2, the partially peeled PNRs are further peeled off by the tape-PDMS contact peeling method to obtain separated and independent PNRs on PDMS; S3, transferring the PNRs on the PDMS to the substrate by a conventional dry transfer method to obtain a substrate with PNRs fixed thereon; S4. Soaking the substrate with the PNRs fixed thereon in an organic solvent and then drying it to obtain phosphorene nanoribbons.
2. The method according to claim 1, characterized in that The black phosphorus polycrystalline sample is a crystal with multiple boundary characteristics; the number of multiple peelings is 3 to 5 times.
3. The method according to claim 1, characterized in that The steps of the tape-PDMS contact stripping method are: The tape carrying the thick BP sheet with partially peeled PNRs was pressed onto the PDMS surface, and then the tape was torn off to achieve further peeling, thereby obtaining separated, independent PNRs on the PDMS.
4. The method according to claim 1, characterized in that: In step S2, the thickness of the PNRs of the PDMS is 1 nm to 100 nm, the width is 15 nm to 1 μm, and the length is 1 μm to 70 μm.
5. The method according to claim 1, characterized in that The dry transfer step is: pressing the PDMS with separated and independent PNRs onto a substrate and keeping it at 40-65° C. for 5-10 minutes, and then separating the PDMS and the substrate; the substrate is a rigid substrate or a flexible substrate.
6. The method according to claim 5, characterized in that The rigid substrate includes one of a Si substrate, a SiO2 / Si substrate, a ceramic substrate and an ITO conductive glass; the flexible substrate includes a polyamide resin film or a polyethylene terephthalate resin film.
7. The method according to claim 1, characterized in that The organic solvent includes at least one of alcohol organic solvents, ether organic solvents, ketone organic solvents, benzene ring organic solvents, dimethyl sulfoxide and dimethylformamide; the drying includes one of inert gas air drying, freeze drying and vacuum oven drying.
8. The method according to claim 7, characterized in that The alcohol organic solvent includes at least one of methanol, ethanol and isopropanol; the ether organic solvent includes diethyl ether and / or phenethyl ether; the ketone organic solvent includes acetone and / or N-methylpyrrolidone; the benzene ring organic solvent includes at least one of benzene, toluene and phenol.
9. A phosphorene nanoribbon obtained by the method according to any one of claims 1 to 8.
10. Use of the phosphorene nanoribbon as claimed in claim 9 in electronic and optoelectronic devices or sensor devices.
Citation Information
Cited By
Method for cleaning interlayer interface in Moire superlattice device construction process
CN120534056A
A cleaning method for interlayer interface in moire superlattice device construction process
CN120534056B