High-performance lithium manganese iron phosphate as well as preparation method and application thereof

By forming a carbon coating layer and a titanium oxide/lithium titanate solid solution coating layer on the surface of lithium manganese iron phosphate, the problems of low conductivity and structural stability of lithium manganese iron phosphate are solved, thereby improving the lithium-ion diffusion rate and the electrochemical performance of the battery.

CN118993014AInactive Publication Date: 2024-11-22WUHAN INSTITUTES OF ADVANCED TECHNOLOGY CHINESE ACADEMY OF SCIENCES
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411166290.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing lithium manganese iron phosphate materials suffer from low conductivity, slow lithium-ion diffusion rate, and structural stability issues, resulting in poor battery electrochemical performance.

Method used

By forming a carbon coating layer on the surface of lithium manganese iron phosphate and combining it with an organic-inorganic hybrid treatment of acidic titanium sol and hydroxy acrylic acid, a titanium oxide/lithium titanate solid solution coating layer is formed, which enhances the conductivity and structural stability of the material.

Benefits of technology

It improves the electronic conductivity and lithium-ion migration rate of lithium manganese iron phosphate, enhances the structural stability and cycle performance of the material, and improves the energy density and long-cycle stability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005007982670000131
    Figure BDA0005007982670000131
  • Figure BDA0005007982670000141
    Figure BDA0005007982670000141
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of lithium manganese iron phosphate materials, in particular to high-performance lithium manganese iron phosphate as well as a preparation method and application thereof. The lithium manganese iron phosphate material provided by the invention is provided with the carbon coating layer, so that the lithium manganese iron phosphate material has relatively good electronic conductivity and rate capability, and the high-temperature performance and the cycle performance are also improved; the acidic titanium sol is added and a titanium oxide / lithium titanate solid solution coating layer is formed, so that the conductivity of the lithium manganese iron phosphate material is improved, and the migration rate and the energy density of lithium ions are improved; due to the addition of the micromolecular hydroxyl acrylic acid substance, the structural stability and conductivity of the prepared lithium manganese iron phosphate material are improved, so that the diffusion rate and energy density of lithium ions are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium manganese iron phosphate material preparation, and in particular to a high-performance lithium manganese iron phosphate and a preparation method and application thereof. Background Art

[0002] Battery technology is a vital part of the storage system of renewable energy and electric devices. As the world pays more attention to environmental protection and sustainable development, the demand for high-performance, environmentally friendly battery materials is also growing. As a new type of positive electrode material, lithium manganese iron phosphate (LiMnFePO4) has attracted much attention due to its high theoretical capacity, excellent thermal stability and good cycle performance. These characteristics make lithium manganese iron phosphate an ideal choice for fields such as electric vehicles and large-scale energy storage systems.

[0003] Traditional methods for preparing lithium manganese iron phosphate include solid-phase synthesis, sol-gel method and hydrothermal method. These methods have achieved certain success on a laboratory scale, but still face many challenges in industrial production. For example, the solid-phase synthesis method usually requires long-term high-temperature calcination, which is not only energy-intensive, but also easily leads to excessive particle growth, affecting the electrochemical properties of the material. Although the sol-gel method can prepare powders with uniform particle size, the process is complicated, the cost is high, and it is difficult to produce on a large scale. The hydrothermal method also has difficulties in controlling the purity and particle size distribution of the product.

[0004] Although lithium manganese iron phosphate materials have a series of significant advantages, such as high thermal stability, environmental friendliness and cost-effectiveness, they also face some defects and challenges in commercial applications. These defects mainly include low electrical conductivity, slow lithium ion diffusion rate, limited energy density and structural stability issues, which in turn lead to poor electrochemical performance of the battery. To overcome these defects, researchers are developing new synthesis methods, doping strategies and composite materials to improve the performance and stability of lithium manganese iron phosphate while reducing costs and environmental impact.

[0005] For example, Chinese patent application CN 105406067A discloses a method for preparing a titanium oxide modified lithium iron manganese phosphate positive electrode material, in which a titanium source is added during the preparation process to eventually form a titanium oxide coating layer, and a carbon source is added to form a carbon layer after carbonization, and the article improves the cycle performance of lithium iron manganese phosphate by coating with titanium oxide without reducing the specific volume. However, the article has the following problems: (1) The structural stability is poor. After a long cycle, the titanium oxide layer is easy to fall off, which reduces the lithium ion migration rate and leads to poor long-term cycle performance of lithium iron manganese phosphate; (2) The high-temperature water bath mechanical stirring is performed until the organic solvent is completely volatilized, which makes the mass production process extremely difficult. Summary of the invention

[0006] The embodiments of the present application provide a high-performance lithium iron manganese phosphate and a preparation method and application thereof to solve the problems of low conductivity, slow lithium ion diffusion rate and structural stability of lithium iron manganese phosphate materials in related technologies, thereby improving the electrochemical performance of the battery, especially the long-cycle stability.

[0007] In a first aspect, a method for preparing high-performance lithium manganese iron phosphate is provided, comprising the following steps:

[0008] Step 1: Mix an iron source, a lithium source, a manganese source, and a phosphorus source to obtain a mixture, add a carbon source and mix well, add an organic solvent, and then obtain carbon-coated lithium manganese iron phosphate after ball milling, sand milling, spray drying, and calcination; in this process, the addition of carbon not only improves the conductivity of the material, but also helps to inhibit the growth of particles, thereby obtaining finer particles and a larger specific surface area;

[0009] Step 2: Mix the carbon-coated lithium manganese iron phosphate, lithium salt and acidic titanium sol, stir them evenly and let them stand, then add hydroxy acrylic acid and mix them evenly and react; the addition of titanium sol can improve the conductivity of the material, and the addition of hydroxy acrylic acid can further optimize the electrochemical properties of the material through organic-inorganic hybridization, and help increase the structural stability after carbonization;

[0010] Step 3: reheating and heat preservation, and finally centrifuging, washing, spray drying and calcining under an inert atmosphere to obtain the high-performance lithium manganese iron phosphate.

[0011] In any embodiment, the molar ratio of the lithium source (calculated as Li), the iron source (calculated as Fe), the manganese source (calculated as Mn), and the phosphorus source (calculated as P) in step 1 is (1.05-1.30):(0.2-0.8):(0.2-0.8):1.

[0012] In any embodiment, the mass ratio of the carbon source to the mixed material in step 1 is (0.001-0.05):1.

[0013] In any embodiment, the organic solvent in step 1 is selected from one of anhydrous ethanol, methanol, isopropanol, acetone and acetic acid.

[0014] In any embodiment, the molar mass ratio of the lithium salt (calculated as Li) to the lithium iron manganese phosphate (calculated as Li) in step 2 is (0.001-0.05):1.

[0015] In any embodiment, the pH value of the acidic titanium sol in step 2 is 5-6.

[0016] In any embodiment, the molar mass ratio of the amount of the acidic titanium sol added to the lithium salt (calculated as Li) added in step 2 is (0.8-1.2):1.

[0017] In any embodiment, the heating and heat preservation in step 3 is performed at a temperature of 100-250° C. and for a time of 2-10 hours.

[0018] In any embodiment, the mass ratio of the amount of hydroxy acrylic acid added in step 2 to the titanium sol is (1-5):1.

[0019] In any embodiment, the standing time in step 2 is 0.5-2 hours, and the reaction time is 3-8 hours.

[0020] In any embodiment, the spray drying temperature in step 3 is 150-300°C.

[0021] In any embodiment, the calcination temperature in step 3 is 500-800° C. and the calcination time is 2-15 hours.

[0022] In any embodiment, the iron source in step 1 is selected from at least one of iron powder, iron oxide, and iron phosphate.

[0023] In any embodiment, the lithium source in step 1 is selected from at least one of lithium carbonate, lithium hydroxide, lithium oxalate, and lithium phosphate.

[0024] In any embodiment, the manganese source is selected from at least one of manganese dioxide, manganese phosphate, and manganese carbonate.

[0025] In any embodiment, the carbon source is selected from at least one of glucose, sucrose, and polyethylene glycol (PEG).

[0026] In any embodiment, the phosphorus source is selected from at least one of phosphoric acid, monoammonium phosphate, and diammonium phosphate.

[0027] The lithium salt in step 2 is selected from at least one of lithium carbonate, lithium oxalate and lithium phosphate.

[0028] In any embodiment, the hydroxy acrylic acid in step 2 is a derivative of acrylic acid, selected from at least one of 3-hydroxypropionic acid, 2-hydroxyethyl acrylate and 2,3-dihydroxypropyl acrylate.

[0029] In a second aspect, the present application provides high-performance lithium manganese iron phosphate prepared using the above method.

[0030] In a third aspect, the present application provides a positive electrode plate, which includes the above-mentioned high-performance lithium manganese iron phosphate.

[0031] In a fourth aspect, the present application provides a battery, comprising the above-mentioned positive electrode plate of the present application.

[0032] The beneficial effects of the technical solution provided by this application include:

[0033] In the preparation process of lithium iron manganese phosphate, the present application first adds a carbon source to form a carbon coating layer, then adds an acidic titanium oxide sol, and acid-etches the obtained lithium iron manganese phosphate to form a microstructure on the surface of the prepared spherical lithium iron manganese phosphate to increase the roughness, provide an anchor point for the titanium oxide / lithium titanate solid solution formed by the titanium oxide sol, and preliminarily increase the adhesion strength of the titanium oxide / lithium titanate solid solution coating layer on the surface of the lithium iron manganese phosphate; then, in the acidic environment provided by the acidic titanium sol, the added small molecule hydroxy acrylic acid reacts with the titanium sol through a hydroxyl cross-linking reaction, and after drying and carbonization, the hydroxy acrylic acid is carbonized to form a carbon coating layer, and the outer surface layer of the titanium oxide / lithium titanate solid solution coating layer formed contains carbon particles, which enhances the adhesion strength of the carbon coating layer on the surface of the material; and the carbon layer formed after the carbonization of the small molecule hydroxy acrylic acid is more uniform and dense, further increasing the structural stability of the material;

[0034] The lithium iron manganese phosphate material prepared in the present application has good electronic conductivity and rate performance due to the carbon coating layer, and also improves the cycle performance; due to the addition of acidic titanium sol and the formation of titanium oxide / lithium titanate solid solution coating layer, the conductivity of the lithium iron manganese phosphate material is further improved, thereby improving the migration rate and energy density of lithium ions; due to the addition of small molecule hydroxy acrylic substances, the structural stability and conductivity of the prepared lithium iron manganese phosphate material are improved, thereby improving the lithium ion diffusion rate and energy density. DETAILED DESCRIPTION

[0035] The technical solution of the present application will be clearly and completely described below in conjunction with the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present application.

[0036] In a first aspect, a method for preparing high-performance lithium manganese iron phosphate is provided, comprising the following steps:

[0037] Step 1: Mix an iron source, a lithium source, a manganese source, and a phosphorus source to obtain a mixture, add a carbon source and mix well, add an organic solvent, and then obtain carbon-coated lithium manganese iron phosphate after ball milling, sand milling, spray drying, and calcination; in this process, the addition of carbon not only improves the conductivity of the material, but also helps to inhibit the growth of particles, thereby obtaining finer particles and a larger specific surface area;

[0038] Step 2: Mix the carbon-coated lithium manganese iron phosphate, lithium salt and acidic titanium sol, stir them evenly and let them stand, then add hydroxy acrylic acid and mix them evenly and react; the addition of titanium sol can improve the conductivity of the material, and the addition of hydroxy acrylic acid can further optimize the electrochemical properties of the material through organic-inorganic hybridization, and help increase the structural stability after carbonization;

[0039] Step 3: reheating and heat preservation, and finally centrifuging, washing, spray drying and calcining under an inert atmosphere to obtain the high-performance lithium manganese iron phosphate.

[0040] In any embodiment, the molar ratio of the lithium source (calculated as Li), the iron source (calculated as Fe), the manganese source (calculated as Mn), and the phosphorus source (calculated as P) in step 1 is (1.05-1.30):(0.2-0.8):(0.2-0.8):1, for example, 1.05:0.2:0.2:1, 1.3:0.2:0.2:1, 1.05:0.8:0.2:1, 1.3:0.8:0.2:1, 1.05:0.2:0.8:1, 1.8:0.2:0.8:1.

[0041] In any embodiment, the mass ratio of the carbon source to the mixed material in step 1 is (0.001-0.05):1, for example, 0.001:1, 0.01:1, 0.03:1, 0.05:1.

[0042] In any embodiment, the organic solvent in step 1 is selected from one of anhydrous ethanol, methanol, isopropanol, acetone and acetic acid.

[0043] In any embodiment, the molar mass ratio of the lithium salt (calculated as Li) to the lithium iron manganese phosphate (calculated as Li) in step 2 is (0.001-0.05):1, for example, 0.001:1, 0.01:1, 0.03:1, 0.05:1.

[0044] In any embodiment, the pH value of the acidic titanium sol in step 2 is 5-6, for example, 5, 5.5, 6; controlling the acidic environment can not only meet the acidic conditions of subsequent reactions, but also slightly etch the surface of the generated carbon-coated lithium manganese iron phosphate through the weak acid environment in this step, and too much acidity will destroy the structure of the carbon-coated lithium manganese iron phosphate.

[0045] In any embodiment, the molar mass ratio of the added amount of the acidic titanium sol to the lithium salt (calculated as Li) added in step 2 is (0.8-1.2):1, for example, 0.8:1, 0.9:1, 1:1, 1.1:1, 1.2:1.

[0046] In any embodiment, the heating and heat preservation in step 3 is performed at a temperature of 100-250° C. (eg, 100° C., 150° C., 200° C., 250° C.) and for a time of 2-10 h (eg, 2 h, 4 h, 6 h, 8 h, 10 h).

[0047] In any embodiment, the mass ratio of the amount of hydroxy acrylic acid added in step 2 to the titanium sol is (1-5):1, for example, 1:1, 2:1, 3:1, 4:1, 5:1.

[0048] In any embodiment, the standing time in step 2 is 0.5-2 h, such as 0.5 h, 1 h, 1.5 h, 2 h; the reaction time is 3-8 h, such as 3 h, 5 h, 8 h.

[0049] In any embodiment, the spray drying temperature in step 3 is 150-300°C, 150°C, 200°C, 250°C, 300°C.

[0050] In any embodiment, the calcination temperature in step 3 is 500-800° C. (eg, 500° C., 600° C., 700° C., 800° C.), and the calcination time is 2-15 h (eg, 2 h, 6 h, 10 h, 15 h).

[0051] In any embodiment, the iron source in step 1 is selected from at least one of iron powder, iron oxide, and iron phosphate.

[0052] In any embodiment, the lithium source in step 1 is selected from at least one of lithium carbonate, lithium hydroxide, lithium oxalate, and lithium phosphate.

[0053] In any embodiment, the manganese source is selected from at least one of manganese dioxide, manganese phosphate, and manganese carbonate.

[0054] In any embodiment, the carbon source is selected from at least one of glucose, sucrose, and polyethylene glycol (PEG).

[0055] In any embodiment, the phosphorus source is selected from at least one of phosphoric acid, monoammonium phosphate, and diammonium phosphate.

[0056] In any embodiment, the lithium salt in step 2 is selected from at least one of lithium carbonate, lithium hydroxide, lithium oxalate, and lithium phosphate.

[0057] In any embodiment, the hydroxy acrylic acid in step 2 is a derivative of acrylic acid, selected from at least one of 3-hydroxypropionic acid, 2-hydroxyethyl acrylate and 2,3-dihydroxypropyl acrylate.

[0058] In a second aspect, the present application provides a high-performance lithium manganese iron phosphate.

[0059] The lithium manganese iron phosphate provided in the present application contains a carbon layer, a titanium oxide / lithium titanate solid solution coating layer and a carbon layer in sequence from the inside to the outside, and the structure has excellent conductivity and structural stability.

[0060] In a third aspect, the present application provides a positive electrode plate, which includes the high-performance lithium iron manganese phosphate provided in the second aspect of the present application.

[0061] The positive electrode plate provided in the present application includes a current collector and a positive electrode film layer arranged on at least one surface of the current collector, and the positive electrode film layer is prepared by a conventional method; an exemplary preparation method includes: mixing the high-performance lithium manganese iron phosphate, a binder, and a conductive agent of the second aspect of the present application, and then coating it on the current collector, and drying it; the mass ratio of lithium manganese iron phosphate, PVDF, and conductive carbon black SP is 9:0.5:0.5.

[0062] In a fourth aspect, the present application provides a battery, comprising the positive electrode plate provided in the third aspect of the present application.

[0063] The battery of the present application may be a lithium-ion battery.

[0064] Furthermore, the battery of the present application can be prepared using conventional methods; in any embodiment, the battery is prepared by assembling the above-mentioned positive electrode sheet, negative electrode sheet, separator, and electrolyte. Exemplary preparation methods include:

[0065] Step 1: stack the positive electrode sheet, negative electrode sheet and separator in order, and wind them to obtain an electrode assembly;

[0066] Step 2: placing the obtained electrode assembly in a secondary battery shell, injecting electrolyte after drying, and then undergoing formation and static processes to obtain a secondary battery.

[0067] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used are not specified by manufacturer and are all conventional products that can be obtained commercially.

[0068] The titanium sol manufacturer involved in the examples and comparative examples of the present application is Xuancheng Jingrui New Materials Co., Ltd.

[0069] Example 1

[0070] Preparation of lithium manganese iron phosphate:

[0071] Step 1, lithium carbonate (calculated as Li), ferrous oxalate (calculated as Fe), manganese dioxide (calculated as Mn), and phosphoric acid (calculated as P) are weighed and mixed to obtain a mixture in a molar ratio of 1.15:0.4:0.6:1, glucose is added in a mass ratio of glucose to the above mixture of 0.02:1, and mixed, anhydrous ethanol is added, and then ball milling and sand milling are performed to reduce the particle size so that the median D50 is less than 300nm, spray drying is performed at 200°C, and then calcining is performed at 600°C for 8h to obtain carbon-coated lithium manganese iron phosphate;

[0072] Step 2, according to the molar mass ratio of lithium carbonate (calculated as Li) and carbon-coated lithium manganese iron phosphate (calculated as Li) of 0.001:1 and the molar mass ratio of acidic titanium sol to lithium carbonate (calculated as Li) of 1:1, the carbon-coated lithium manganese iron phosphate, lithium carbonate and acidic titanium sol (pH value is 5.5) are mixed and stirred evenly and then allowed to stand for 1 hour, and then 3-hydroxypropionic acid is added according to the mass ratio of 3-hydroxypropionic acid to titanium sol of 3:1, mixed and reacted for 5 hours;

[0073] Step 3, heating at 100° C. and keeping the temperature for 10 hours, and finally centrifuging, washing, spray drying at 300° C. and calcining at 720° C. for 10 hours under an inert atmosphere to obtain the high-performance lithium manganese iron phosphate.

[0074] Example 2

[0075] Preparation of lithium manganese iron phosphate:

[0076] Step 1, lithium hydroxide (calculated as Li), iron powder (calculated as Fe), manganese phosphate (calculated as Mn), and monoammonium phosphate (calculated as P) are weighed and mixed to obtain a mixture in a molar ratio of 1.05:0.7:0.3:1, sucrose is added in a mass ratio of sucrose to the above-mentioned mixture of 0.001:1, and the mixture is mixed evenly, and methanol is added and then ball milled and sand milled to reduce the particle size so that the median D50 is less than 300 nm, spray dried at 200° C., and calcined at 600° C. for 8 h to obtain carbon-coated lithium manganese iron phosphate;

[0077] Step 2, according to the molar mass ratio of lithium carbonate (calculated as Li) to carbon-coated lithium manganese iron phosphate (calculated as Li) of 0.05:1 and the molar mass ratio of acidic titanium sol to lithium carbonate (calculated as Li) of 0.8:1, the carbon-coated lithium manganese iron phosphate, lithium carbonate and acidic titanium sol (pH value is 5) are mixed and stirred evenly, and then allowed to stand for 0.5h, and then 2-hydroxyethyl acrylic acid is added according to the mass ratio of 2-hydroxyethyl acrylic acid to titanium sol of 1:1, mixed evenly and reacted for 3h;

[0078] Step 3, heating at 150° C. and keeping the temperature for 6 hours, and finally centrifuging, washing, spray drying at 180° C. and calcining at 500° C. for 15 hours under an inert atmosphere to obtain the high-performance lithium manganese iron phosphate.

[0079] Example 3

[0080] Preparation of lithium manganese iron phosphate:

[0081] Step 1, lithium oxalate (calculated as Li), iron oxide (calculated as Fe), manganese carbonate (calculated as Mn), and diammonium phosphate (calculated as P) are weighed and mixed to obtain a mixture in a molar ratio of 1.30:0.4:0.6:1, polyethylene glycol is added in a mass ratio of polyethylene glycol to the above-mentioned mixture of 0.05:1, and the mixture is mixed evenly, isopropanol is added, and the mixture is ball-milled and sand-milled to reduce the particle size so that the median D50 is less than 300 nm, spray-dried at 200° C., and calcined at 600° C. for 8 h to obtain carbon-coated lithium manganese iron phosphate;

[0082] Step 2, according to the molar mass ratio of lithium oxalate (calculated as Li) to the above-mentioned lithium manganese iron phosphate (calculated as Li) of 0.05:1 and the molar mass ratio of acidic titanium sol to lithium oxalate (calculated as Li) of 1.2:1, the carbon-coated lithium manganese iron phosphate, lithium oxalate and acidic titanium sol (pH value is 6) are mixed and stirred evenly and then allowed to stand for 2 hours, and then 2,3-dihydroxypropyl acrylate is added according to the mass ratio of 2,3-dihydroxypropyl acrylate to titanium sol of 5:1, mixed and reacted for 8 hours;

[0083] Step 3, heating at 250° C. and keeping the temperature for 2 hours, and finally centrifuging, washing, spray drying at 300° C. and calcining at 800° C. for 2 hours under an inert atmosphere to obtain the high-performance lithium manganese iron phosphate.

[0084] Example 4

[0085] Preparation of lithium manganese iron phosphate:

[0086] Step 1, lithium phosphate (calculated as Li), iron phosphate (calculated as Fe), manganese dioxide (calculated as Mn), phosphoric acid (calculated as P) are weighed and mixed to obtain a mixture in a molar ratio of 1.05:0.4:0.6:1, glucose is added in a mass ratio of glucose to the above mixture of 0.03:1, and is mixed, isopropanol is added, and the mixture is ball-milled and sand-milled to reduce the particle size so that the median D50 is less than 300 nm, spray-dried at 200° C., and calcined at 600° C. for 8 h to obtain carbon-coated lithium manganese iron phosphate;

[0087] Step 2, according to the molar mass ratio of lithium phosphate (calculated as Li) and carbon-coated lithium manganese iron phosphate (calculated as Li) of 0.01:1 and the molar mass ratio of acidic titanium sol to lithium phosphate (calculated as Li) of 1:1, the carbon-coated lithium manganese iron phosphate, lithium phosphate and acidic titanium sol (pH value is 5.5) are mixed and stirred evenly, and then allowed to stand for 1 hour, and then 3-hydroxypropionic acid is added according to the mass ratio of 3-hydroxypropionic acid to titanium sol of 2:1, mixed and reacted for 5 hours;

[0088] Step 3, heating at 150° C. and keeping the temperature for 6 hours, and finally centrifuging, washing, spray drying at 300° C. and calcining at 720° C. for 10 hours under an inert atmosphere to obtain the high-performance lithium manganese iron phosphate.

[0089] Comparative Example 1

[0090] Preparation of lithium manganese iron phosphate:

[0091] Step 1, lithium carbonate (calculated as Li), ferrous oxalate (calculated as Fe), manganese dioxide (calculated as Mn), phosphoric acid (calculated as P) are weighed and mixed to obtain a mixture in a molar ratio of 1.15:0.4:0.6:1, glucose is added in a mass ratio of glucose to the above mixture of 0.02:1, and the mixture is mixed, anhydrous ethanol is added, and the mixture is ball-milled and sand-milled to reduce the particle size so that the median D50 is less than 300 nm, and the mixture is spray-dried at 200° C., and then calcined at 600° C. for 8 h to obtain carbon-coated lithium manganese iron phosphate;

[0092] Step 2, mixing the carbon-coated lithium manganese iron phosphate and lithium carbonate in a molar mass ratio of lithium carbonate (calculated as Li) to carbon-coated lithium manganese iron phosphate (calculated as Li) of 0.001:1, stirring evenly and standing for 1 hour, then adding 3-hydroxypropionic acid in a mass ratio of 3-hydroxypropionic acid to the lithium carbonate added in step 2 of 3:1, mixing evenly and reacting for 5 hours;

[0093] Step 3, heating at 100° C. and keeping the temperature for 10 hours, and finally centrifuging, washing, spray drying at 300° C. and calcining at 720° C. for 10 hours under an inert atmosphere to obtain the high-performance lithium manganese iron phosphate.

[0094] Comparative Example 2

[0095] Preparation of lithium manganese iron phosphate:

[0096] Step 1, lithium carbonate (calculated as Li), ferrous oxalate (calculated as Fe), manganese dioxide (calculated as Mn), and phosphoric acid (calculated as P) are weighed and mixed to obtain a mixture in a molar ratio of 1.15:0.4:0.6:1, glucose is added in a mass ratio of glucose to the above mixture of 0.02:1, and mixed, anhydrous ethanol is added, and then the mixture is ball-milled and sand-milled to reduce the particle size so that the median D50 is less than 300 nm, spray-dried at 200° C., and calcined at 600° C. for 8 hours to obtain carbon-coated lithium manganese iron phosphate;

[0097] Step 2, according to the molar mass ratio of lithium carbonate (calculated as Li) to carbon-coated lithium manganese iron phosphate (calculated as Li) of 0.001:1 and the molar mass ratio of acidic titanium sol to lithium carbonate (calculated as Li) of 1:1, the carbon-coated lithium manganese iron phosphate, lithium carbonate and acidic titanium sol (pH value of 5.5) were mixed and stirred evenly and then allowed to stand for 1 hour;

[0098] Step 3, heating at 100° C. and keeping the temperature for 10 hours, and finally centrifuging, washing, spray drying at 300° C. and calcining at 720° C. under an inert atmosphere for 10 hours to obtain the high-performance lithium manganese iron phosphate.

[0099] Comparative Example 3

[0100] Preparation of lithium manganese iron phosphate:

[0101] Step 1, lithium carbonate (calculated as Li), ferrous oxalate (calculated as Fe), manganese dioxide (calculated as Mn), and phosphoric acid (calculated as P) are weighed and mixed to obtain a mixture in a molar ratio of 1.15:0.4:0.6:1, glucose is added in a mass ratio of glucose to the above mixture of 0.02:1, and mixed, anhydrous ethanol is added, and then the mixture is ball-milled and sand-milled to reduce the particle size so that the median D50 is less than 300 nm, spray-dried at 200° C., and calcined at 600° C. for 8 hours to obtain carbon-coated lithium manganese iron phosphate;

[0102] Step 2, according to the molar mass ratio of lithium carbonate (calculated as Li) to carbon-coated lithium manganese iron phosphate (calculated as Li) of 0.001:1 and the molar mass ratio of acidic titanium sol to lithium carbonate (calculated as Li) of 1:1, the carbon-coated lithium manganese iron phosphate, lithium carbonate and acidic titanium sol (pH value is 5.5) are mixed and stirred evenly and then allowed to stand for 1 hour, and then polyacrylic acid (McLean: P761913) is added according to the mass ratio of polyacrylic acid to titanium sol of 3:1, mixed and reacted for 5 hours;

[0103] Step 3, heating at 100° C. and keeping the temperature for 10 hours, and finally centrifuging, washing, spray drying at 300° C. and calcining at 720° C. for 10 hours under an inert atmosphere to obtain the high-performance lithium manganese iron phosphate.

[0104] Performance Testing

[0105] The lithium manganese iron phosphate obtained in the embodiment and the comparative example is prepared into a button battery. The preparation process is divided into two parts, namely, the preparation of the positive electrode sheet and the preparation of the battery, specifically:

[0106] 1. Positive electrode sheet preparation process: First weigh a certain amount of N-methylpyrrolidone (NMP), then stir PVDF in it for 6 hours, then add the above-mentioned lithium manganese iron phosphate and acetylene black and continue stirring for 6 hours. The mixed slurry is stirred and mixed evenly by a magnetic stirrer and then coated on a smooth aluminum foil. Use scrapers of different thicknesses to scrape out the corresponding different thicknesses and uniform materials on the smooth aluminum foil. Vacuum in a vacuum drying oven and set the temperature to 120°C. After drying for 12 hours, the prepared electrode sheet is obtained. The electrode sheet is cut into 14mm discs using a tablet press to obtain a positive electrode sheet;

[0107] 2. Battery assembly process: Place the coated positive electrode sheet in the positive electrode shell and drip an appropriate amount of electrolyte, the electrolyte is 1MLiPF6 (ethylene carbonate: dimethyl carbonate volume ratio is 1:1); then place the diaphragm and drip an equal amount of electrolyte, and then place the lithium sheet, steel sheet and shrapnel in turn; then buckle the negative electrode shell on it, and then use a sealing machine to package it into a CR 2032 button battery; the above assembly procedures are all completed in an argon-filled glove box (water oxygen values ​​are all less than 0.01ppm).

[0108] Finally, the CR 2032 button battery was left to stand for 24 hours before the performance test. The CR 2032 button battery was tested by placing it on a battery tester. The test was conducted at 25℃±2℃. The voltage range of the CR 2032 button battery was 2.0-4.5V during the test. The final test results are shown in Table 1.

[0109] Table 1

[0110]

[0111]

[0112] From the test results of the embodiments and comparative examples, it can be seen that the addition of acidic titanium sol to form a titanium oxide / lithium titanate solid solution coating layer and small molecule hydroxyacrylate to form a carbon coating layer in the embodiments can not only improve the capacity of iron manganese ferrophosphate, but also stabilize the structure and improve the battery cycle stability; the comparative example does not add acidic titanium sol or small molecule hydroxyacrylate, cannot effectively improve the conductivity, electrical conductivity and structural stability, and the rate performance and cycle performance are relatively poor.

Claims

1. A method for preparing high-performance lithium manganese iron phosphate, characterized in that: The following steps are involved: Step 1, mixing an iron source, a lithium source, a manganese source, and a phosphorus source to obtain a mixture, adding a carbon source and mixing evenly, adding an organic solvent, and then ball milling, sand milling, spray drying, and calcining to obtain carbon-coated lithium manganese iron phosphate; Step 2, mixing the carbon-coated lithium manganese iron phosphate, lithium salt and acidic titanium sol, stirring them evenly and letting them stand, and then adding hydroxy acrylic acid, mixing them evenly and reacting them; Step 3: reheating and heat preservation treatment, and finally centrifuging, washing, spray drying and calcining under an inert atmosphere to obtain the high-performance lithium manganese iron phosphate.

2. The method for preparing high-performance lithium iron manganese phosphate according to claim 1, characterized in that: The molar ratio of the lithium source (calculated as Li), the iron source (calculated as Fe), the manganese source (calculated as Mn), and the phosphorus source (calculated as P) in step 1 is (1.05-1.30):(0.2-0.8):(0.2-0.8):

1.

3. The method for preparing high-performance lithium iron manganese phosphate according to claim 1, characterized in that: The mass ratio of the carbon source to the mixed material in step 1 is (0.001-0.05):

1.

4. The method for preparing high-performance lithium iron manganese phosphate according to claim 1, characterized in that: The molar mass ratio of the lithium salt (calculated as Li) to the lithium iron manganese phosphate (calculated as Li) in step 2 is (0.001-0.05):

1.

5. The method for preparing high-performance lithium iron manganese phosphate according to claim 1, characterized in that: The pH value of the acidic titanium sol in step 2 is 5-6.

6. The method for preparing high-performance lithium iron manganese phosphate according to claim 1, characterized in that: The molar mass ratio of the amount of the acidic titanium sol added in step 2 to the lithium salt (calculated as Li) added in step 2 is (0.8-1.2):

1.

7. The method for preparing high-performance lithium iron manganese phosphate according to claim 1, characterized in that: The mass ratio of the added amount of hydroxy acrylic acid to the titanium sol in step 2 is (1-5):

1.

8. The method for preparing high-performance lithium iron manganese phosphate according to claim 1, characterized in that: The hydroxy acrylic acid in step 2 is a derivative of acrylic acid, and is selected from at least one of 3-hydroxypropionic acid, 2-hydroxyethyl acrylate and 2,3-dihydroxypropyl acrylate.

9. A high-performance lithium manganese iron phosphate prepared according to the method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of carbon-coated lithium titanate negative electrode material

    CN111668467A

  • Preparation method of coated modified lithium iron manganese phosphate positive electrode material

    CN116581266A

  • Titanium-modified lithium iron manganese phosphate-based material as well as preparation method and application thereof

    CN117976849A

  • Carbon-coated lithium manganese iron phosphate material as well as preparation method and application thereof

    CN117996049A

  • Lithium manganese iron phosphate positive active material as well as preparation method and application thereof

    CN118016875A