Preparation method of Ni and Zn bimetallic ZIF-8 derived carbon material with electromagnetic wave absorption performance

By introducing nickel ions into the ZIF-8 framework, Ni and Zn bimetallic ZIF-8 derived carbon materials with multiple losses mechanisms are formed, and the problem of insufficient electromagnetic wave absorption performance in the prior art is solved, and wide-band and efficient electromagnetic wave absorption is achieved Effects are suitable for the needs of new electromagnetic wave absorbing materials.

CN118993025APending Publication Date: 2024-11-22HARBIN INST OF TECH AT WEIHAI
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411089217.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing ZIF-8 derived carbon materials have problems such as a single electromagnetic wave loss mechanism, poor polarization capability and poor impedance matching performance, and it is difficult to meet the requirements of "thin, light, wide and strong" electromagnetic wave absorption performance.

Method used

By introducing nickel ions into the ZIF-8 frame structure, a square plane coordination with a unique d8 electronic configuration is formed, resulting in structural defects and multiple loss mechanisms, enhancing electromagnetic wave loss capability, and achieving mediation through the ratio adjustment of nickel ions to zinc ions The coordination between electrical and magnetic losses is complementary.

Benefits of technology

It significantly improves the electromagnetic wave absorption performance, achieves wide-band and efficient electromagnetic wave absorption, reduces reflection and scattering phenomena, meets the needs of new electromagnetic wave absorption materials, and is simple in preparation, cheap and easy to obtain, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993025A_ABST
    Figure CN118993025A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of nano carbon-based composite materials, and relates to a preparation method of a Ni and Zn bimetallic ZIF-8 derived carbon material with electromagnetic wave absorption performance. Metal nickel is introduced when the ZIF-8 wave-absorbing material is constructed, and a defect structure is introduced into a ZIF-8 three-dimensional organic framework structure through square plane coordination guided by a unique d8 electron configuration of nickel ions to form a regular tetrakaidecahedron morphology different from a typical regular dodecahedron. Meanwhile, a magnetic loss mechanism is introduced on the basis of dielectric loss, and the dissipation capacity of electromagnetic waves is enhanced. The impedance matching characteristic of the sample can be improved due to the high specific surface area and the ordered pore structure of the ZIF-8, so that electromagnetic waves can enter the sample more easily, and the reflection and scattering phenomena of the electromagnetic waves in the sample are enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nano carbon-based composite materials, and in particular to a method for preparing a Ni, Zn bimetallic ZIF-8 derived carbon material with electromagnetic wave absorption performance. Background Art

[0002] At present, wireless communication technology, mainly 5G networks, is developing rapidly. The derived smart devices have brought great convenience to people's lives, but also made the electromagnetic environment of society more and more complex. In order to solve the negative impact of electromagnetic interference, people focus on electromagnetic wave absorbing materials. Traditional electromagnetic wave absorbing materials such as ferrites, metal particles and other magnetic loss materials have the disadvantages of poor acid and alkali resistance, high density, large matching thickness and easy oxidation; dielectric loss materials such as carbon nanotubes and graphene have the disadvantages of easy oxidation, poor impedance matching, narrow absorption bandwidth, etc., which cannot meet the current performance requirements of electromagnetic wave absorbing materials of "thin, light, wide and strong". Therefore, in order to solve the shortcomings of the above-mentioned single electromagnetic wave absorbing materials, composite materials have gradually come into people's field of vision.

[0003] Zeolitic Imidazolate Framework (ZIF) is a highly ordered, spatially regular three-dimensional porous material formed by self-assembly of metal ions and imidazole compounds through chemical bonds. It has the advantages of high specific surface area, adjustable pore structure, good chemical stability and thermal stability, and easy chemical modification, and has broad application prospects.

[0004] However, existing ZIF-8 derived carbon materials have the following technical problems:

[0005] (1) The electromagnetic wave loss mechanism is single. Multiple loss mechanisms can enhance the electromagnetic wave dissipation path and improve the overall performance, while the effect of a single loss mechanism is greatly reduced.

[0006] (2) Poor polarization ability: the more defects a sample has, the stronger its dipole polarization ability and the stronger its electromagnetic wave absorption performance. However, due to the thermal stability of ZIF materials, it has few defects and poor polarization ability.

[0007] (3) Poor impedance matching performance and high conductivity will produce a strong skin effect, generating surface current to prevent electromagnetic waves from entering the interior of the material. Summary of the invention

[0008] The purpose of the present invention is to provide a method for preparing a Ni, Zn bimetallic ZIF-8 derived carbon material with electromagnetic wave absorption performance, by preparing a carbon material derived from a ZIF-8 organic-inorganic hybrid framework structure with rich defect structure and uniformly dispersed Ni and Zn bimetallics, so as to solve the problems existing in the above-mentioned prior art and achieve excellent electromagnetic wave absorption performance.

[0009] To achieve the above object, the present invention provides the following solutions:

[0010] One of the technical solutions of the present invention is to provide a method for preparing a Ni, Zn bimetallic ZIF-8 derived carbon material having electromagnetic wave absorption performance, the steps comprising:

[0011] Using dimethylimidazole as an organic ligand and soluble zinc salt and soluble nickel salt as metal sources, Ni, Zn bimetallic ZIF-8 was prepared;

[0012] The Ni, Zn bimetallic ZIF-8 is calcined under an inert atmosphere to obtain the Ni, Zn bimetallic ZIF-8 derived carbon material.

[0013] Furthermore, the molar ratio of the organic ligand to the metal source is 1:8-10, preferably 1:9.

[0014] Furthermore, the molar ratio of the soluble zinc salt to the soluble nickel salt is 9-3:1-2, preferably 7:3.

[0015] Furthermore, the soluble zinc salt is Zn(CH3COOH)2·2H2O and / or Zn(NO3)2·6H2O, preferably Zn(CH3COOH)2·2H2O.

[0016] Furthermore, the soluble nickel salt is Ni(CH3COOH)2·4H2O and / or Ni(NO3)2·6H2O, preferably Ni(CH3COOH)2·4H2O.

[0017] Furthermore, the steps of preparing Ni and Zn bimetallic ZIF-8 include:

[0018] Dissolving dimethylimidazole in water to obtain an organic ligand solution;

[0019] dissolving a soluble zinc salt and a soluble nickel salt in water to obtain a metal source solution;

[0020] The metal source solution is slowly added into the organic ligand solution, and the Ni, Zn bimetallic ZIF-8 is obtained through stirring, standing, centrifugal solid-liquid separation, washing and drying.

[0021] In the above further embodiment, the dimethylimidazole is dissolved in water and the soluble zinc salt and the soluble nickel salt are dissolved in water, wherein the amount of water used can completely dissolve the aforementioned solutes, which meets the requirements of the present invention.

[0022] Preferably, the stirring time is 0.5 to 1 h; the standing time is 3 to 24 h; the rotation speed of the centrifugal solid-liquid separation is 8000 to 10000 rpm, and the time is 4 to 10 min; the drying temperature is 80 to 120° C., and the time is 12 to 24 h.

[0023] More preferably, the stirring time is 1 hour; the standing time is 12 hours; the rotation speed of the centrifugal solid-liquid separation is 10000 rpm, and the time is 5 minutes; the drying temperature is 80°C, and the time is 24 hours.

[0024] Furthermore, the inert atmosphere is a nitrogen atmosphere or an argon atmosphere.

[0025] Furthermore, the calcination temperature is 550-750° C., the heating rate is 2-5° C. / min, and the calcination time is 2-5 h.

[0026] Preferably, the calcination temperature is 750° C., the heating rate is 3° C. / min, and the calcination time is 3 h.

[0027] The second technical solution of the present invention is to provide a Ni, Zn bimetallic ZIF-8 derived carbon material obtained by the above preparation method.

[0028] Conventional ZIF-8 materials are mainly composed of zinc ions and dimethylimidazole for coordination and complexation. The electromagnetic wave loss mechanism of the carbon materials derived from them is single and the impedance matching characteristics are poor. The present invention introduces the magnetic element nickel into the ZIF-8 framework structure, and then uses the unique d 8 The square plane coordination guided by the electronic configuration introduces structural defects in the three-dimensional organic framework structure, resulting in a tetradecahedron morphology different from the typical regular dodecahedron. In addition, the derived carbon material adds a magnetic loss mechanism to the single dielectric loss mechanism, further enhancing the electromagnetic wave loss path of the material. The structural defects caused by nickel ions can also induce the generation of polarization phenomena, enhancing the electromagnetic wave loss capacity of the material. At the same time, the ratio of nickel ions to zinc ions is highly adjustable, and the dielectric loss capacity and magnetic loss capacity of the composite material can be adjusted according to different application scenarios, so as to achieve the synergistic complementarity of dielectric loss and magnetic loss to improve the absorbing performance of the composite absorbing material and its tolerance to high working intensity, which provides a new idea for improving the performance of ZIF composite materials. At the same time, the material preparation method is simple, the raw material price is low, and it is easy to apply on a large scale.

[0029] The third technical solution of the present invention is to provide an application of the above-mentioned Ni, Zn bimetallic ZIF-8 derived carbon material in improving the electromagnetic wave absorption performance of the electromagnetic wave absorber.

[0030] The fourth technical solution of the present invention is to provide an electromagnetic wave absorbing composite material, wherein the composite material has paraffin as a matrix and the above-mentioned Ni, Zn bimetallic ZIF-8 derived carbon material as a filler.

[0031] Furthermore, the filling amount of the filler in the composite material is 30-40wt%, and the filling thickness is 2.5-4.0mm.

[0032] The present invention discloses the following technical effects:

[0033] The invention can significantly improve the typical regular dodecahedron morphology of ZIF-8 under the introduction of nickel ions, and prepare ZIF-8 with a regular tetradecahedron morphology by taking advantage of the incompatibility of nickel ions with the three-dimensional organic framework.

[0034] The present invention introduces nickel ions into the framework structure of ZIF-8. The unique d 8 The electronic configuration-adapted square plane coordination can introduce defects in the three-dimensional framework structure, forming a tetradecahedron morphology that is different from the typical regular dodecahedron, and the derived carbon material has stronger polarization properties. At the same time, nickel, as a magnetic metal, can introduce a magnetic loss mechanism on the dielectric loss, and multiple loss mechanisms give the material excellent electromagnetic wave loss capacity. ZIF-8 has an extremely high specific surface area and an ordered three-dimensional pore structure. The formation of cavities can significantly improve the impedance matching characteristics of the sample, making it easier for electromagnetic waves to enter the interior of the sample, thereby reducing the reflection and scattering of electromagnetic waves and improving the strong skin effect of carbon materials. In addition, the preparation method has high stability, strong controllability, simple steps, and cheap and easy-to-obtain raw materials, which is conducive to large-scale production. The prepared Ni, Zn bimetallic ZIF-8-derived carbon material can meet the requirements of "thin, light, wide, and strong" electromagnetic wave absorbers and has broad application prospects.

[0035] Under the condition of a low filling ratio of 40wt%, the effective absorption bandwidth of the synthesized composite material can reach 4.92GHz at a matching thickness of 2.8mm; at 9.04GHz, the minimum reflection loss can reach -42.14dB (matching thickness 4.4mm). The present invention has the excellent performance of broadband, strong reflection loss and matching thickness, meeting the needs of new electromagnetic wave absorption materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0037] Figure 1 The X-ray diffraction pattern of the Ni, Zn bimetallic ZIF-8 prepared in step S3 of Example 1;

[0038] Figure 2 The scanning electron microscope images of the Ni, Zn bimetallic ZIF-8 prepared in Examples 1 to 4, wherein (a) is Example 1, (b) is Example 2, (c) is Example 3, and (d) is Example 4;

[0039] Figure 3 This is a scanning electron microscope image of the pure Zn single metal ZIF-8 prepared in Comparative Example 4;

[0040] Figure 4 The scanning electron microscope images of the Ni, Zn bimetallic ZIF-8 derived carbon materials prepared in Example 3 and Comparative Example 3, wherein (a) is Example 3, and (b) is Comparative Example 3;

[0041] Figure 5 The electromagnetic parameter diagram of the Ni, Zn bimetallic ZIF-8 derived carbon material prepared in Example 3, wherein (a) is a distribution diagram of the real part of dielectric loss ε′, (b) is a distribution diagram of the imaginary part of dielectric loss ε″, (c) is a distribution diagram of magnetic loss μ′, (d) is a distribution diagram of magnetic loss μ″, (e) is a distribution diagram of dielectric loss tangent, (f) is a distribution diagram of magnetic loss tangent, (g) is a Cole-Cole circle distribution diagram, and (h) is an impedance matching distribution diagram;

[0042] Figure 6 A three-dimensional graph showing the variation of reflection loss with frequency at different thicknesses of the Ni and Zn bimetallic ZIF-8 derived carbon material in Example 3 in the prepared electromagnetic wave absorbing composite material;

[0043] Figure 7 This is a two-dimensional graph of the reflection loss of the Ni and Zn bimetallic ZIF-8 derived carbon material in Example 3 as a function of frequency at different thicknesses in the prepared electromagnetic wave absorbing composite material. DETAILED DESCRIPTION

[0044] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0045] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0046] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0047] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0048] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0049] Unless otherwise specified, the room temperature and normal temperature referred to in the specific embodiments of the present invention refer to 20-30°C.

[0050] Example 1

[0051] Preparation steps of Ni, Zn bimetallic ZIF-8 derived carbon materials:

[0052] S1. Weigh 6 g of dimethylimidazole (organic ligand) and dissolve it in 20 mL of deionized water and stir for 1 h to obtain a clear and uniform organic ligand solution;

[0053] S2, weigh 1.62g Zn(CH3COOH)2·2H2O and 0.21g Ni(CH3COOH)2·4H2O (metal source, molar ratio 9:1) and dissolve them in 10mL deionized water and stir for 1h to obtain a clear and uniform metal source solution;

[0054] S3. Slowly add the metal source solution to the organic ligand solution, continue stirring for 1 hour to make it uniformly mixed, and form a light gray-blue suspension. Then, let it stand for 12 hours, collect the obtained lavender solid by high-speed centrifuge (10000 rpm centrifugation for 5 minutes), wash it with anhydrous ethanol solution for 4 times, and dry it in a blast oven at 80°C for 24 hours to obtain Ni, Zn bimetallic ZIF-8;

[0055] S4. The Ni, Zn bimetallic ZIF-8 was calcined at 750°C for 3 h in a tubular furnace under a nitrogen atmosphere at a heating rate of 3°C / min to obtain a Ni, Zn bimetallic ZIF-8 derived carbon material.

[0056] The Ni and Zn bimetallic ZIF-8 derived carbon material prepared in this embodiment was filled into a paraffin matrix to obtain an electromagnetic wave absorbing composite material. The filling amount was 40wt%. The minimum reflection loss of the electromagnetic wave absorbing composite material was measured to be -20.35dB, the matching thickness corresponding to the minimum reflection loss was 5.5mm, and the effective bandwidth below -10dB was 2.58GHz.

[0057] Example 2

[0058] Compared with Example 1, the only difference is that the molar ratio of Zn(CH3COOH)2·2H2O and Ni(CH3COOH)2·4H2O is 4:1, that is, the amount of Zn(CH3COOH)2·2H2O is 1.44g, and the amount of Ni(CH3COOH)2·4H2O is 0.41g.

[0059] The Ni and Zn bimetallic ZIF-8 derived carbon material prepared in this embodiment was filled into a paraffin matrix to obtain an electromagnetic wave absorbing composite material. The filling amount was 40wt%. The minimum reflection loss of the electromagnetic wave absorbing composite material was measured to be -29.68dB, the matching thickness corresponding to the minimum reflection loss was 4.9mm, and the effective bandwidth below -10dB was 3.47GHz.

[0060] Example 3

[0061] Compared with Example 1, the only difference is that the molar ratio of Zn(CH3COOH)2·2H2O and Ni(CH3COOH)2·4H2O is 7:3, that is, the amount of Zn(CH3COOH)2·2H2O is 1.26g, and the amount of Ni(CH3COOH)2·4H2O is 0.61g.

[0062] The Ni and Zn bimetallic ZIF-8 derived carbon material prepared in this embodiment was filled into a paraffin matrix to obtain an electromagnetic wave absorbing composite material, with a filling amount of 40wt%. The minimum reflection loss of the electromagnetic wave absorbing composite material was measured to be -42.14dB, the matching thickness corresponding to the minimum reflection loss was 4.4mm, and the effective bandwidth below -10dB was 4.96GHz, which met the requirements of lightweight and high efficiency of electromagnetic wave absorbing materials.

[0063] Example 4

[0064] Compared with Example 1, the only difference is that the molar ratio of Zn(CH3COOH)2·2H2O and Ni(CH3COOH)2·4H2O is 3:2, that is, the amount of Zn(CH3COOH)2·2H2O is 1.08 g, and the amount of Ni(CH3COOH)2·4H2O is 0.82 g.

[0065] The Ni and Zn bimetallic ZIF-8 derived carbon material prepared in this embodiment was filled into a paraffin matrix to obtain an electromagnetic wave absorbing composite material. The filling amount was 40wt%. The minimum reflection loss of the electromagnetic wave absorbing composite material was measured to be -35.77dB, the matching thickness corresponding to the minimum reflection loss was 3.9mm, and the effective bandwidth below -10dB was 3.29GHz.

[0066] Example 5

[0067] Compared with Example 3, the only difference is that the molar ratio of the metal source to the organic ligand is 1:8.

[0068] The Ni and Zn bimetallic ZIF-8 derived carbon material prepared in this embodiment was filled into a paraffin matrix to obtain an electromagnetic wave absorbing composite material. The filling amount was 40wt%. The minimum reflection loss of the electromagnetic wave absorbing composite material was measured to be -23.59dB, the matching thickness corresponding to the minimum reflection loss was 4.5mm, and the effective bandwidth below -10dB was 3.83GHz.

[0069] Example 6

[0070] Compared with Example 3, the only difference is that the molar ratio of the metal source to the organic ligand is 1:10.

[0071] The Ni and Zn bimetallic ZIF-8 derived carbon material prepared in this embodiment was filled into a paraffin matrix to obtain an electromagnetic wave absorbing composite material. The filling amount was 40wt%. The minimum reflection loss of the electromagnetic wave absorbing composite material was measured to be -29.70dB, the matching thickness corresponding to the minimum reflection loss was 3.8mm, and the effective bandwidth below -10dB was 3.45GHz.

[0072] Comparative Example 1

[0073] Compared with Example 3, the only difference is that the centrifugal rotation speed in step S3 is 6000 rpm.

[0074] Due to the reduction in centrifugal speed, the precipitated product is not effectively separated and the quality of the product is reduced.

[0075] Comparative Example 2

[0076] Compared with Example 1, the difference is that the metal sources selected are Zn(NO3)2·6H2O and Ni(NO3)2·6H2O.

[0077] The Ni and Zn bimetallic ZIF-8 derived carbon material prepared in this comparative example was filled into a paraffin matrix to obtain an electromagnetic wave absorbing composite material. The filling amount was 40wt%. The minimum reflection loss of the electromagnetic wave absorbing composite material was measured to be -30.51dB, the matching thickness corresponding to the minimum reflection loss was 3.8mm, and the effective bandwidth below -10dB was 3.74GHz.

[0078] Comparative Example 3

[0079] Compared with Example 3, the difference is that the calcination temperature in step S4 is 900° C. and the calcination time is 36 hours.

[0080] The Ni and Zn bimetallic ZIF-8 derived carbon material prepared in this comparative example was filled into a paraffin matrix to obtain an electromagnetic wave absorbing composite material, with a filling amount of 40wt%. The minimum reflection loss of the electromagnetic wave absorbing composite material was measured to be -12.61dB, the matching thickness corresponding to the minimum reflection loss was 4.9mm, and the effective bandwidth below -10dB was 2.05GHz.

[0081] The calcination temperature is too high, which destroys the structure of the derived carbon material and leads to a significant decrease in the microwave absorption performance.

[0082] Comparative Example 4

[0083] Compared with Example 3, the only difference is that the metal source is a single Zn(CH3COOH)2·2H2O, and the ratio of the metal source to the organic ligand remains unchanged.

[0084] The ZIF-8 derived carbon material prepared in this comparative example was filled into a paraffin matrix to prepare an electromagnetic wave absorbing composite material, with a filling amount of 40wt%. The minimum reflection loss of the electromagnetic wave absorbing composite material was measured to be -23.59dB, the matching thickness corresponding to the minimum reflection loss was 4.2mm, and the effective bandwidth below -10dB was 3.83GHz.

[0085] Due to the lack of nickel elements, the material has poor wave absorption performance.

[0086] Figure 1 This is the X-ray diffraction pattern of the Ni, Zn bimetallic ZIF-8 prepared in step S3 of Example 1. Figure 1 It can be seen that pure phase ZIF-8 can be synthesized under this condition.

[0087] Figure 2 The scanning electron microscope images of the Ni, Zn bimetallic ZIF-8 prepared in Examples 1 to 4 are shown in Figures 1 to 4, where (a) is Example 1, (b) is Example 2, (c) is Example 3, and (d) is Example 4. Figure 2 It can be seen that in (a) and (b), ZIF-8 gradually changes from a regular dodecahedron to a regular tetradecahedron as the nickel content increases; when the molar ratio is 7:3, the material just changes to a regular tetradecahedron, as shown in (c); as the nickel content further increases, the surface morphology of the material gradually changes from a regular tetradecahedron to a smooth sphere, as shown in (d), and its microstructure is affected by the incorporation of nickel. At the same time, as the nickel content gradually increases, its wave absorption performance first increases and then decreases. The molar ratio of zinc to nickel with the best wave absorption performance is 7:3. This is because under this ratio, the amount of nickel introduced is the largest while preserving the complete microstructure. RL≤-10dB is called effective wave absorption. The smaller the RL value, the better the wave absorption performance of this material.

[0088] Figure 3 This is a scanning electron microscope image of the pure Zn single metal ZIF-8 prepared in Comparative Example 4. Figure 3 It can be seen that the sample morphology of pure Zn single metal ZIF-8 without nickel doping is a regular dodecahedron.

[0089] Figure 4 The scanning electron microscope images of the ZIF-8 derived carbon materials after carbonization in Example 3 and Comparative Example 3 are shown in FIG. (a) is Example 3 and (b) is Comparative Example 3. Figure 4 It can be seen that when the calcination temperature is too high, the structure of the derived carbon material is destroyed.

[0090] Figure 5 The electromagnetic parameter diagram of the Ni, Zn bimetallic ZIF-8 derived carbon material prepared in Example 3, wherein (a) is the distribution diagram of the real part of dielectric loss ε′, (b) is the distribution diagram of the imaginary part of dielectric loss ε″, (c) is the distribution diagram of magnetic loss μ′, (d) is the distribution diagram of magnetic loss μ″, (e) is the distribution diagram of dielectric loss tangent, (f) is the distribution diagram of magnetic loss tangent, (g) is the Cole-Cole circle distribution diagram, and (h) is the impedance matching distribution diagram. Figure 5It can be seen that nickel doping enhances magnetic loss and realizes the dual loss mechanism of the material. As can be seen from (g), there are four semicircles with different diameters in the material, indicating the existence of multiple polarization relaxation phenomena in the system. Nickel doping increases the defects of the sample and enhances the dipole polarization ability, thereby enhancing the electromagnetic wave absorption performance compared with the pure ZIF-8 in comparative example 4. As can be seen from (h), the impedance matching performance is good, and the skin effect produced will prevent electromagnetic waves from entering the interior of the material, so that the sample of Example 3 has good wave absorption performance.

[0091] Figure 6 is a three-dimensional graph showing the variation of reflection loss with frequency at different thicknesses of the Ni and Zn bimetallic ZIF-8 derived carbon material in Example 3 in the prepared electromagnetic wave absorbing composite material, Figure 6 It can be seen that when the thickness is 4.4 mm, the optimal reflection loss value is -42.14 dB.

[0092] Figure 7 is a two-dimensional graph of the reflection loss of the Ni and Zn bimetallic ZIF-8 derived carbon material in Example 3 at different thicknesses in the prepared electromagnetic wave absorbing composite material as a function of frequency, Figure 7 It can be seen that within the thickness range of 2.0-6.0 mm and the frequency range of 4.16-18 GHz, the optimal reflection loss values ​​are all lower than -10 dB, and can cover the C band, X band and Ku band.

[0093] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing a Ni, Zn bimetallic ZIF-8 derived carbon material with electromagnetic wave absorption performance, It is characterized in that the steps include: Using dimethylimidazole as an organic ligand and soluble zinc salt and soluble nickel salt as metal sources, Ni, Zn bimetallic ZIF-8 was prepared; The Ni, Zn bimetallic ZIF-8 is calcined under an inert atmosphere to obtain the Ni, Zn bimetallic ZIF-8 derived carbon material.

2. The preparation method according to claim 1, It is characterized in that The molar ratio of the organic ligand to the metal source is 1:8-10; the molar ratio of the soluble zinc salt to the soluble nickel salt is 9-3:1-2.

3. The preparation method according to claim 1, It is characterized in that The soluble zinc salt is Zn(CH 3 COOH) 2 ·2H 2 O and / or Zn(NO 3 ) 2 6H 2 O; the soluble nickel salt is Ni(CH 3 COOH) 2 ·4H 2 O and / or Ni(NO 3 ) 2 6H 2 O.

4. The preparation method according to claim 1, It is characterized in that The steps of preparing Ni, Zn bimetallic ZIF-8 include: Dissolving dimethylimidazole in water to obtain an organic ligand solution; dissolving a soluble zinc salt and a soluble nickel salt in water to obtain a metal source solution; The metal source solution is slowly added into the organic ligand solution, and the Ni, Zn bimetallic ZIF-8 is obtained through stirring, standing, centrifugal solid-liquid separation, washing and drying.

5. The preparation method according to claim 4, It is characterized in that The stirring time is 0.5 to 1 hour; the standing time is 3 to 24 hours; the rotation speed of the centrifugal solid-liquid separation is 8000 to 10000 rpm, and the time is 4 to 10 minutes; the drying temperature is 80 to 120° C., and the time is 12 to 24 hours.

6. The preparation method according to claim 1, It is characterized in that The inert atmosphere is a nitrogen atmosphere or an argon atmosphere.

7. The preparation method according to claim 1, It is characterized in that The calcination temperature is 550-750° C., the heating rate is 2-5° C. / min, and the calcination time is 2-5 hours.

8. A Ni, Zn bimetallic ZIF-8 derived carbon material obtained by the preparation method according to any one of claims 1 to 7.

9. Use of the Ni, Zn bimetallic ZIF-8 derived carbon material according to claim 8 in improving the electromagnetic wave absorption performance of an electromagnetic wave absorber.

10. An electromagnetic wave absorbing composite material, It is characterized in that The composite material uses paraffin as a matrix and the Ni, Zn bimetallic ZIF-8 derived carbon material described in claim 8 as a filler.

Citation Information

Patent Citations

  • Ni-N-C catalyst for electroreduction reaction of carbon dioxide and preparation and application thereof

    CN109652821A

  • Hollow carbon-loaded metallic nickel particles, preparation method and application of hollow carbon-loaded metallic nickel particles in microwave absorption

    CN115843172A

  • Nickel-zinc nanocapsule / nanoflower composite wave-absorbing material with corrosion resistance and preparation method of nickel-zinc nanocapsule / nanoflower composite wave-absorbing material

    CN116355587A

  • Multi-metal MOF-derived composite nitrogen-doped carbon material film, preparation method and application thereof