Preparation method and application of bimodal pore size distribution porous carbon
By combining modified polyacrylonitrile with polyvinyl alcohol copolymer and carboxyl-containing polypyridine and using inorganic base, the problem of uneven pore size distribution of porous carbon is solved, and bimodal pore size with high porosity and specific surface area is achieved The distribution of porous carbon significantly improves the adsorption performance of precious metals.
Patent Information
- Application Number
- CN202411096016.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-12
AI Technical Summary
The pore size distribution of existing pores is uneven, resulting in insufficient adsorption capacity of precious metals, and the commonly used preparation methods are complex and costly.
Modified with polyacrylonitrile-polyvinyl alcohol diblock copolymer and carboxyl-containing polypyridine to form a linear-body block polymer, and the bimodal pore size distribution is achieved through the carbonization process, combined with the use of inorganic bases to improve porosity and specific surface area.
The prepared bimodal pore size distribution porous carbon has a more concentrated and high porosity and specific surface area, which significantly improves the adsorption performance of precious metals.
Smart Images

Figure CN118993027A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of porous carbon, and in particular relates to a preparation method and application of porous carbon with bimodal pore size distribution. Background Art
[0002] Precious metal resources are scarce and expensive; precious metals in secondary resources mainly come from electronic waste, printed circuit boards, and wastewater generated during jewelry processing; therefore, from the perspective of saving resources and protecting the environment, the recycling of precious metal secondary resources is of great significance. Currently, the commonly used methods for precious metal recovery are ion exchange, extraction, chemical precipitation, electrolysis, and adsorption; among them, adsorption is more efficient and environmentally friendly than other methods. Porous carbon is the main adsorbent used in the adsorption method due to its rich pores and high specific surface area; however, the pore distribution of conventional porous carbon is uneven and the pore size is single, so its adsorption capacity for precious metals is insufficient. According to the International Union of Pure and Applied Chemistry, pores with a pore size less than 2nm are micropores, pores with a pore size greater than 50nm are macropores, and those in between are called mesopores. The porous carbon with the two above-mentioned different pore size ranges concentratedly distributed (double peaks appearing in the pore size distribution diagram) is a bimodal pore size distribution porous carbon. The synergistic effect of pores of different sizes can overcome the shortcomings of a single pore structure. Therefore, its specific surface area and volume utilization are higher, and it also shows greater advantages in the field of secondary resource recovery of precious metals.
[0003] At present, the methods for preparing porous carbon with bimodal pore size distribution mainly include activation method and template method. The activation method can prepare porous carbon with higher specific surface area, but the pore size distribution is generally wider. The template method is divided into inorganic template method and organic template method. In the inorganic template method, the carbon precursor is introduced into the molecular sieve template, and the bimodal porous carbon is prepared through carbonization and template removal. This method requires the synthesis of molecular sieve templates. The preparation process of the template itself is complicated, the raw materials used are expensive, and the adjustable range of pore size is limited. The organic template method is to mix two organic compounds with different thermal stability, and only prepare bimodal porous carbon through carbonization. This method has a simple preparation process, but the pore size distribution is not concentrated and the pore distribution is uneven.
[0004] Wang Yu et al. (Acta Physico-Chimica Sinica, 2012, 28: 1525-1532) used long rod-shaped γ-alumina with a large difference between the stacking pore size and its own diameter as a template and in-situ polymerized phenolic resin as a carbon source. They prepared a thin-walled carbon material with a bimodal pore distribution structure through polymerization-carbonization. The two peaks were located in the smaller mesopore area near 4nm and the larger mesopore area near 13nm, respectively. However, the pore size distribution near 4nm is not concentrated. Summary of the invention
[0005] In view of the above problems, an object of the present invention is to provide a method for preparing a porous carbon with a bimodal pore size distribution. The prepared porous carbon with a bimodal pore size distribution has a concentrated pore size distribution and has a high porosity and specific surface area.
[0006] The present invention adopts the following technical solutions to achieve the above purpose:
[0007] A method for preparing porous carbon with bimodal pore size distribution comprises the following steps:
[0008] (S1) uniformly mixing polyacrylonitrile-polyvinyl alcohol diblock copolymer (PAN-PVA), carboxyl-containing polypyridine, and a stabilizer, and heating the mixture for reaction to obtain modified polyacrylonitrile; the PVA segment portion in the PAN-PVA accounts for 8 to 15 wt %; and the mass ratio of the PAN-PVA to the carboxyl-containing polypyridine is 100:(20 to 40);
[0009] (S2) dissolving modified polyacrylonitrile and polyvinyl pyrrolidone in an organic solvent at a mass ratio of 100:(10-30) to form a polymer solution; dropping the polymer solution into water at room temperature to precipitate solid pellets, filtering and drying to obtain solid pellets;
[0010] (S3) After mixing the solid beads with an inorganic base, carbonizing under an inert atmosphere, cooling, washing with water, and drying, a porous carbon with a bimodal pore size distribution is obtained.
[0011] The diblock copolymer (PAN-PVA) formed by polyacrylonitrile and polyvinyl alcohol is a linear AB-type block polymer containing hydroxyl groups, where A is a polyacrylonitrile segment and B is a polyvinyl alcohol segment. When PAN-PVA is modified by carboxyl-containing polypyridine, the carboxyl group in the carboxyl-containing polypyridine reacts with the hydroxyl group in the B segment to form an interpenetrating cross-linked structure; at the same time, the interpenetrating cross-linked structure contains a polypyridine structure, and the pyridine group is a nitrogen-containing heterocyclic structure. The polypyridine structure has relatively good thermal stability. The modified polyacrylonitrile finally formed is a linear-stereotype block polymer, where the linear molecular chain is a polyacrylonitrile segment and the stereotype part is a cross-linked structure containing polypyridine; the polypyridine structure and the interpenetrating cross-linked structure work together to make the modified polyacrylonitrile have better thermal stability. Modified polyacrylonitrile with better thermal stability decomposes at about 400°C, while polyvinylpyrrolidone has a lower decomposition temperature and can decompose at 250-300°C; that is, the two decompose at different temperatures in the subsequent carbonization stage to produce small molecules that escape from the matrix, thereby achieving graded pore formation and forming porous carbon with two different pore size ranges, namely, bimodal pore size distribution porous carbon. Since modified polyacrylonitrile is a linear-block polymer formed in situ, it realizes molecular-scale block and cross-linking, which not only has a more concentrated pore size distribution but also a high porosity.
[0012] The proportion of PVA chain segments and the proportion of carboxyl-containing polypyridine in PAN-PVA must be controlled within a certain range. If the dosage is too low, the interpenetrating cross-linking structure will have fewer connection points, the thermal stability of the modified polyacrylonitrile will be limited, and the graded pore formation will not be obvious; if the dosage is too high, the overall carbonization rate of the product will be reduced.
[0013] Furthermore, in step (S1), the carboxyl-containing polypyridine is at least one of poly(pyridine-2-acetic acid), poly(pyridine-3-acetic acid), poly(pyridine-4-acetic acid), poly(pyridine-2-carboxylic acid), poly(pyridine-3-carboxylic acid), poly(pyridine-4-carboxylic acid), and poly(6-methoxy-3-pyridineacetic acid); and its number average molecular weight is 3000 to 5000.
[0014] Furthermore, in step (S1), the number average molecular weight of the PAN-PVA is 50,000 to 80,000, and the PAN-PVA can be homemade or commercially available.
[0015] Furthermore, in step (S1), the stabilizer is trimethyl phosphate, and its usage is 0.1 to 0.3 wt % of PAN-PVA.
[0016] Furthermore, in step (S1), the heating reaction is: adding PAN-PVA and carboxyl-containing polypyridine into a horizontal twin-screw mixer, heating to 50-70°C, and mixing at medium speed for 20-40 minutes; then adding a stabilizer thereto, heating to 180-190°C, and mixing at high speed for 30-50 minutes.
[0017] Further, in step (S1), the carboxyl-containing polypyridine is prepared by a method comprising the following steps:
[0018] (L1) dissolving a pyridinate ester in an organic solvent, adding an oxidant under N2 protection, stirring and reacting at 0-5°C for 5-8h to obtain a reactant; then pouring the reactant into an alcohol solvent, standing, filtering, washing and drying to obtain a polypyridinate ester;
[0019] (L2) adding polypyridinate to an aqueous solution of an inorganic base to undergo a hydrolysis reaction at 90-100° C.; then adding hydrochloric acid to obtain a precipitate, filtering, washing, and drying to obtain a carboxyl-containing polypyridine.
[0020] Preferably, in step (L1), the molar ratio of the pyridinic acid ester to the oxidant is 1:(1.2-2.5).
[0021] Preferably, in step (L1), the pyridinate ester is at least one of methyl pyridine-2-acetate, methyl pyridine-3-acetate, methyl polypyridine-4-acetate, ethyl pyridine-2-carboxylate, ethyl pyridine-3-carboxylate, ethyl pyridine-4-carboxylate, and methyl 6-methoxy-3-pyridineacetate; the organic solvent is at least one of chloroform, carbon tetrachloride, and dichloromethane; the oxidant is at least one of FeCl3, MoCl5, and RuCl3; the alcohol solvent is at least one of methanol, ethanol, and isopropanol; and the washing and drying is washing with water 2 to 3 times and then vacuum drying at 50 to 60°C for 10 to 24 hours.
[0022] Preferably, in step (L2), the molar ratio of the pyrrolidone group to the inorganic base in the polypyrrolidone ester is 1:(1.1-1.3).
[0023] Preferably, in step (L2), the inorganic base is NaOH or KOH, and the concentration of its aqueous solution is 1-2 mol / L; the hydrolysis reaction is a hydrolysis reaction for 12-24 hours; the concentration of the hydrochloric acid solution is 1-2 mol / L, and the amount of hydrochloric acid used is adjusted to a pH of 5-6; the washing and drying is washing with water 2-3 times and then vacuum drying at 50-60°C for 10-24 hours.
[0024] Furthermore, in step (S2), the number average molecular weight of the polyvinyl pyrrolidone is 1000-5000; the organic solvent is at least one of N,N-dimethylformamide (DMF) and N,N-dimethylacetamide (DMA); the concentration of the polymer solution is 10wt%-15wt%. If the polymer concentration is too high, it is not easy to drip in, and if the polymer concentration is too low, it is not easy to form solid pellets, and the yield is low. Dissolving and mixing the modified polyacrylonitrile and polyvinyl pyrrolidone and then making solid pellets can make the two fully mixed at the molecular level, which is conducive to improving the uniformity and specific surface area of the pores in the subsequent carbonization.
[0025] Furthermore, in step (S2), the polymer solution is dripped at a speed of 10 to 20 mL / h. The dripping speed affects the particle size of the solid spheres. The slower the dripping speed, the smaller the particle size of the solid spheres. The smaller the particle size of the solid spheres, the smaller the pore size formed after carbonization, the larger the pore volume, and the larger the specific surface area. On the contrary, the larger the particle size, the smaller the specific surface area of the porous carbon obtained. Considering the efficiency and performance, the dripping speed is controlled within a certain range.
[0026] Furthermore, in step (S3), the mass ratio of the solid beads to the inorganic base is 100:(30-50), and the inorganic base is KOH and / or NaOH. As an activator, the inorganic base has a strong dehydration and intercalation effect, which is conducive to the porous carbon to produce a rich pore structure, thereby increasing its specific surface area.
[0027] Furthermore, in step (S3), the inert atmosphere is at least one of nitrogen, argon and helium; and the carbonization conditions are: heating to 700-900°C at a heating rate of 3-8°C / min and keeping warm for 3-8h.
[0028] Furthermore, in step (S3), the water washing is performed by washing with deionized water until the mixture becomes neutral; and the drying is performed in an oven at 80 to 120° C. for 24 to 36 hours.
[0029] In a second aspect, the present invention provides the use of the porous carbon with bimodal pore size distribution prepared by the above preparation method in the recovery of precious metals.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] (1) The present invention uses carboxyl-containing polypyridine to modify PAN-PVA to obtain a modified polyacrylonitrile with a linear-block structure, which has better thermal stability and decomposes at about 400°C; while polyvinyl pyrrolidone has a lower decomposition temperature, decomposing at 250-300°C; the two decompose at different temperatures in the subsequent carbonization stage to produce small molecules that escape from the matrix, thereby achieving graded pore formation, that is, forming a porous carbon with a bimodal pore size distribution. Since the modified polyacrylonitrile is an in-situ formed linear-block polymer, molecular-scale block and cross-linking are achieved, not only the pore size distribution is more concentrated but also the porosity is high.
[0032] (2) The pore sizes of the bimodal pore size distribution porous carbon prepared by the present invention are concentrated in 2-3 nm and 9-12 nm, respectively, and have high porosity and specific surface area; the two different sizes of pores work synergistically to show strong adsorption performance for precious metals. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is the pore size distribution diagram of the bimodal pore size distribution porous carbon prepared in Example 1. DETAILED DESCRIPTION
[0034] In order to better explain the present invention, the following description will be given in detail with reference to the embodiments of the present invention, and the main contents of the present invention will be further clarified in conjunction with specific examples. However, the contents of the present invention are not limited to the following examples.
[0035] Unless otherwise specified, the "parts" in the examples of the present invention are all parts by weight. All reagents used are commercially available reagents in the art.
[0036] Polyacrylonitrile-polyvinyl alcohol diblock copolymer (PAN-PVA) was purchased from Xi'an Ruixi Biotechnology Co., Ltd., the PVA segment portion of which accounted for about 12 wt %, and the number average molecular weight of PAN-PVA was about 65,000.
[0037] Polyvinyl pyrrolidone was purchased from Aladdin Reagent Co., Ltd., and its number average molecular weight was about 3,000.
[0038] Polyacrylonitrile (PAN) was purchased from Beijing Bailingwei Technology Co., Ltd., and the number average molecular weight was about 58,000.
[0039] Preparation of polypyridine containing carboxyl groups
[0040] Preparation Example 1
[0041] (L1) 4.53 g (30 mmol) of methyl pyridine-2-acetate was dissolved in 200 mL of chloroform, and 9.73 g (60 mmol, i.e., the molar ratio of pyridine ester to oxidant was 1:2) of anhydrous FeCl3 was added under N2 protection, and the mixture was stirred and reacted at 2±1°C for 6 h to obtain a reactant; the reactant was then poured into an ethanol solvent, allowed to stand and filtered, washed twice with pure water, and dried at 60°C for 12 h to obtain poly(methyl pyridine-2-acetate);
[0042] (L2) Add all the poly(methyl pyridine-2-acetate) prepared in step (L1) into 36 mL of 1 mol / L NaOH aqueous solution (36 mmol of NaOH), and perform hydrolysis reaction at 100° C. for 12 h; then add 1 mol / L hydrochloric acid solution to adjust the pH of the system to 5.5 to obtain a precipitate, which is filtered, washed with pure water twice, and dried at 60° C. for 12 h to obtain poly(pyridine-2-acetic acid).
[0043] The number average molecular weight of poly(pyridine-2-acetic acid) was determined to be about 4,000 by gel permeation chromatography.
[0044] Preparation Example 2
[0045] (L1) 4.53 g (30 mmol) of ethyl pyridine-3-carboxylate was dissolved in 200 mL of chloroform, and 9.84 g (36 mmol, i.e., the molar ratio of pyridine ester to oxidant was 1:1.2) of anhydrous MoCl5 was added under N2 protection, and the mixture was stirred at 0°C for 5 h to obtain a reactant; the reactant was then poured into an ethanol solvent, allowed to stand and filtered, washed twice with pure water, and dried at 60°C for 12 h to obtain poly(ethyl pyridine-3-carboxylate);
[0046] (L2) Add all the poly(ethyl pyridine-3-carboxylate) prepared in step (L1) into 36 mL of 1 mol / L NaOH aqueous solution (36 mmol of NaOH), and carry out hydrolysis reaction at 100°C for 12 hours; then add 1 mol / L hydrochloric acid solution to adjust the pH of the system to 5.5 to obtain a precipitate, which is filtered, washed with pure water twice, and dried at 60°C for 12 hours to obtain poly(pyridine-3-carboxylic acid).
[0047] The number average molecular weight of poly(pyridine-3-carboxylic acid) was about 2500 as determined by gel permeation chromatography.
[0048] Preparation Example 3
[0049] The rest is the same as Example 1, except that in step (L1), methyl pyridine-4-acetate is used instead of methyl pyridine-2-acetate, and the reaction is stirred at 4±1°C for 8h; finally, poly(pyridine-4-acetic acid) is obtained. The number average molecular weight of poly(pyridine-4-acetic acid) is about 5500 as determined by gel permeation chromatography.
[0050] Example 1
[0051] (S1) adding 100 parts of polyacrylonitrile-polyvinyl alcohol diblock copolymer (PAN-PVA) and 20 parts of poly(pyridine-2-acetic acid) obtained in Preparation Example 1 into a horizontal twin-screw mixer, heating to 50-70° C., mixing at medium speed for 30 minutes, then adding 0.1 parts of stabilizer trimethyl phosphate, heating to 180° C., mixing at high speed for 40 minutes, extruding and cooling, to obtain modified polyacrylonitrile;
[0052] (S2) dissolving 100 parts of modified polyacrylonitrile and 10 parts of polyvinyl pyrrolidone in 800 parts of N,N-dimethylformamide (DMF) to form a polymer solution with a concentration of 12 wt%; transferring the polymer solution to a propeller, dripping it into water at room temperature at 15 mL / h, and solid pellets precipitating out, filtering and drying to obtain solid pellets;
[0053] (S3) After mixing 100 parts of solid beads with 30 parts of NaOH, the temperature was raised to 700°C at 5°C / min in an argon atmosphere and kept warm for 6 hours; carbonized, cooled, washed with deionized water until neutral, and dried in an oven at 100°C for 24 hours to obtain a porous carbon with a bimodal pore size distribution.
[0054] Example 2
[0055] The rest is the same as Example 1, except that in step (S1), the poly(pyridine-3-carboxylic acid) prepared in Preparation Example 2 is used instead of the poly(pyridine-2-acetic acid) prepared in Preparation Example 1.
[0056] Example 3
[0057] The rest is the same as Example 1, except that in step (S1), the poly(pyridine-4-acetic acid) prepared in Preparation Example 3 is used instead of the poly(pyridine-2-acetic acid) prepared in Preparation Example 1.
[0058] Example 4
[0059] The rest is the same as implementation 1, except that:
[0060] The amount of each material used in step (S1) is different, specifically: 100 parts of PAN-PVA, 30 parts of poly(pyridine-2-acetic acid) prepared in Preparation Example 1;
[0061] The amount of each material used in step (S1) is different, specifically: 100 parts of modified polyacrylonitrile and 20 parts of polyvinyl pyrrolidone.
[0062] Example 5
[0063] The rest is the same as implementation 1, except that:
[0064] The amount of each material used in step (S1) is different, specifically: 100 parts of PAN-PVA, 30 parts of poly(pyridine-2-acetic acid) prepared in Preparation Example 1;
[0065] The amount of each material used in step (S1) is different, specifically: 100 parts of modified polyacrylonitrile and 30 parts of polyvinyl pyrrolidone.
[0066] Example 6
[0067] The rest is the same as implementation 1, except that:
[0068] The amount of each material used in step (S1) is different, specifically: 100 parts of PAN-PVA, 40 parts of poly(pyridine-2-acetic acid) prepared in Preparation Example 1;
[0069] The amount of each material used in step (S1) is different, specifically: 100 parts of modified polyacrylonitrile and 30 parts of polyvinyl pyrrolidone.
[0070] Comparative Example 1
[0071] The rest is the same as in Embodiment 1, except that step (S1) is omitted, that is, carboxyl-containing polypyridine is not used to modify PAN-PVA, that is:
[0072] (1) dissolving 100 parts of PAN-PVA and 10 parts of polyvinyl pyrrolidone in 800 parts of N,N-dimethylformamide (DMF) to form a polymer solution with a concentration of 12 wt%; transferring the polymer solution to a propeller, dripping it into water at room temperature at a rate of 15 mL / h, and solid pellets precipitating out, filtering and drying to obtain solid pellets;
[0073] (2) After mixing 100 parts of solid pellets with 30 parts of NaOH, the mixture was heated to 700°C at a rate of 5°C / min in an argon atmosphere and kept at this temperature for 6 hours; the mixture was carbonized, cooled, washed with deionized water until neutral, and dried in an oven at 100°C for 24 hours to obtain porous carbon.
[0074] Comparative Example 2
[0075] The rest is the same as in Embodiment 1, except that step (S1) is omitted, and polyacrylonitrile (PAN) is used in place of modified polyacrylonitrile in step (S2), namely:
[0076] (1) dissolving 100 parts of PAN and 10 parts of polyvinyl pyrrolidone in 800 parts of N,N-dimethylformamide (DMF) to form a polymer solution with a concentration of 12 wt%; transferring the polymer solution to a propeller, dripping it into water at room temperature at a rate of 15 mL / h, and solid pellets precipitating out, filtering and drying to obtain solid pellets;
[0077] (2) After mixing 100 parts of solid pellets with 30 parts of NaOH, the mixture was heated to 700°C at a rate of 5°C / min in an argon atmosphere and kept at this temperature for 6 hours; the mixture was carbonized, cooled, washed with deionized water until neutral, and dried in an oven at 100°C for 24 hours to obtain porous carbon.
[0078] Testing and analysis
[0079] The porous carbon prepared in the examples and comparative examples was subjected to the following tests:
[0080] (1) Specific surface area and pore size: The porous carbons prepared in the examples and comparative examples were subjected to a low-temperature nitrogen adsorption experiment using a Tristar II 3020 fully automatic specific surface and pore size analyzer produced by Micromeritics Instrument Corporation of the United States to measure the specific surface area and pore size distribution of the porous carbons. The specific data are shown in Table 1.
[0081] Figure 1 This is the pore size distribution diagram of the bimodal pore size distribution porous carbon prepared in Example 1.
[0082] (2) Noble metal ion adsorption test: A platinum ion solution and a palladium ion solution with a pH of 3 and a concentration of 100 mg / L were prepared; 0.08 g of the porous carbon prepared in each embodiment and comparative example was added to 20 mL of the above platinum ion solution and palladium ion solution, respectively, and oscillated and adsorbed at 25° C. and 250 rpm for 3 h; after the adsorption was completed, the solid-liquid separation was performed, and the supernatant was collected. The platinum ion concentration and palladium ion concentration in the supernatant were detected by atomic absorption (AAS), and the adsorption rate was obtained by calculating the concentration difference before and after adsorption. The specific data are shown in Table 2.
[0083]
[0084] Table 1 Specific surface area agent pore size distribution
[0085]
[0086]
[0087] It can be seen from Table 1 that the porous carbon prepared in the embodiment of the present invention has a bimodal pore size distribution, with pore sizes concentrated in 2-3 nm and 9-12 nm respectively; Figure 1 It can be seen that both peaks are relatively narrow, indicating that the pore size distribution is concentrated. However, the porous carbons prepared in Comparative Examples 1 and 2 cannot achieve a bimodal pore size distribution and have a low specific surface area.
[0088] Table 2 Adsorption performance of precious metal ions
[0089] Group Platinum ion absorption rate (%) Palladium ion absorption rate (%) Example 1 99.5 98.8 Example 2 99.3 98.4 Example 3 99.4 98.5 Example 4 99.7 99.2 Example 5 99.6 99.1 Example 6 99.5 99.1 Comparative Example 1 87.2 84.9 Comparative Example 2 81.7 79.8
[0090] It can be seen from Table 2 that the bimodal pore size distribution porous carbon prepared in the embodiment of the present invention has strong adsorption performance for platinum ions and palladium ions, and the adsorption rates for platinum ions and palladium ions are above 99% and 98%, respectively.
[0091] The above detailed description is a specific description of one feasible embodiment of the present invention. The embodiment is not intended to limit the patent scope of the present invention. Any equivalent implementation or modification that does not deviate from the present invention should be included in the scope of the technical solution of the present invention.
Claims
1. A method for preparing porous carbon with bimodal pore size distribution, characterized in that: The following steps are involved: (S1) uniformly mixing polyacrylonitrile-polyvinyl alcohol diblock copolymer (PAN-PVA), carboxyl-containing polypyridine, and a stabilizer, and heating the mixture for reaction to obtain modified polyacrylonitrile; the PVA segment portion in the PAN-PVA accounts for 8 to 15 wt %; and the mass ratio of the PAN-PVA to the carboxyl-containing polypyridine is 100:(20 to 40); (S2) dissolving modified polyacrylonitrile and polyvinyl pyrrolidone in an organic solvent at a mass ratio of 100:(10-30) to form a polymer solution; dropping the polymer solution into water at room temperature to precipitate solid pellets, filtering and drying to obtain solid pellets; (S3) After mixing the solid beads with an inorganic base, carbonizing under an inert atmosphere, cooling, washing with water, and drying, a porous carbon with a bimodal pore size distribution is obtained.
2. The preparation method according to claim 1, characterized in that: In step (S1), the carboxyl-containing polypyridine is at least one of poly(pyridine-2-acetic acid), poly(pyridine-3-acetic acid), poly(pyridine-4-acetic acid), poly(pyridine-2-carboxylic acid), poly(pyridine-3-carboxylic acid), poly(pyridine-4-carboxylic acid), and poly(6-methoxy-3-pyridineacetic acid); and its number average molecular weight is 3000 to 5000.
3. The preparation method according to claim 1, characterized in that: In step (S1), the number average molecular weight of the PAN-PVA is 50,000 to 80,000.
4. The preparation method according to claim 1, characterized in that: In step (S1), the stabilizer is trimethyl phosphate, and its usage is 0.1-0.3wt% of PAN-PVA; the heating reaction is: adding PAN-PVA and carboxyl-containing polypyridine into a horizontal twin-screw mixer, heating to 50-70°C, and mixing at medium speed for 20-40min; then adding the stabilizer thereto, heating to 180-190°C, and mixing at high speed for 30-50min.
5. The preparation method according to claim 1, characterized in that: In step (S1), the carboxyl-containing polypyridine is prepared by a method comprising the following steps: (L1) dissolving a pyridinate ester in an organic solvent, adding an oxidant under N2 protection, stirring and reacting at 0-5°C for 5-8h to obtain a reactant; then pouring the reactant into an alcohol solvent, standing, filtering, washing and drying to obtain a polypyridinate ester; (L2) adding polypyridinate to an aqueous solution of an inorganic base to undergo a hydrolysis reaction at 90-100° C.; then adding hydrochloric acid to obtain a precipitate, filtering, washing, and drying to obtain a carboxyl-containing polypyridine.
6. The preparation method according to claim 5, characterized in that: In step (L1), the molar ratio of the pyridinic acid ester to the oxidant is 1:(1.2-2.5); and / or The pyridinate ester is at least one of pyridine-2-acetic acid methyl ester, pyridine-3-acetic acid methyl ester, polypyridine-4-acetic acid methyl ester, pyridine-2-carboxylic acid ethyl ester, pyridine-3-carboxylic acid ethyl ester, pyridine-4-carboxylic acid ethyl ester, and 6-methoxy-3-pyridineacetic acid methyl ester; the organic solvent is at least one of chloroform, carbon tetrachloride, and dichloromethane; the oxidant is at least one of FeCl3, MoCl5, and RuCl3; the alcohol solvent is at least one of methanol, ethanol, and isopropanol; the washing and drying is washing with water 2 to 3 times and then vacuum drying at 50 to 60°C for 10 to 24 hours.
7. The preparation method according to claim 5, characterized in that: In step (L2), the molar ratio of the pyrrolidone group to the inorganic base in the polypyrrolidone ester is 1:(1.1-1.3).
8. The preparation method according to claim 1, characterized in that: In step (S2), the number average molecular weight of the polyvinyl pyrrolidone is 1000-5000; the organic solvent is at least one of N,N-dimethylformamide (DMF) and N,N-dimethylacetamide (DMA); the concentration of the polymer solution is 10wt%-15wt%; and the dripping rate of the polymer solution is 10-20mL / h.
9. The preparation method according to claim 1, characterized in that: In step (S3), the mass ratio of the solid ball to the inorganic base is 100:(30-50), and the inorganic base is KOH and / or NaOH; the inert atmosphere is at least one of nitrogen, argon, and helium; and the carbonization conditions are: heating to 700-900° C. at a heating rate of 3-8° C. / min and keeping warm for 3-8 hours.
10. Use of the porous carbon with bimodal pore size distribution prepared by the preparation method according to any one of claims 1 to 9 in the recovery of precious metals.
Citation Information
Patent Citations
Method for preparing mesopore-micropore composite porous carbon on basis of vinylidene chloride polymers
CN102807206A
Preparation method of monodisperse nanometer olivine type manganese-based phosphate positive-pole material and lithium-ion secondary battery thereof
CN102810664A
Preparation method of polymer-based porous carbon supercapacitor electrode
CN117059402A
Foamed, adhesion-optimized polymer composition and adhesive bonding
DE202018105677U1
System for Predicting Failure of Automobile Parts
KR1020240060018A