Method and device for preparing nanocrystalline magnesium oxide from salt lake magnesium salt

Through the combination of salt lake magnesium salt preparation and ultrasonic atomization combined with plasma discharge technology, the complexity and environmental protection of synthesis of nanocrystalline magnesium oxide in the existing technology is solved, and efficient and environmentally friendly nanocrystalline magnesium oxide synthesis is achieved under normal temperature and pressure. , provides simple and fast process flow and excellent nanocrystalline MgO ceramic material properties.

CN118993116APending Publication Date: 2024-11-22QINGHAI INST OF SALT LAKES OF CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410978534.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The prior art synthesis of high-purity nanocrystalline magnesium oxide has problems such as complex operation, high equipment requirements, high production costs, large environmental pollution and long process flow, making it difficult to achieve efficient, environmentally friendly and controllable nanocrystalline MgO ceramic materials. Control synthesis.

Method used

The precursor solution is prepared by salt lake magnesium salt, and the aerosol is formed by ultrasonic atomization treatment, and the aerosol is discharged at a preset discharge power in the plasma discharge synthesis unit to synthesize nanocrystalline magnesium oxide.

Benefits of technology

It realizes rapid, simple, green and environmentally friendly nanocrystalline magnesium oxide synthesis under normal temperature and pressure. The reactor structure is simple, can operate stably for a long time, and the product has good crystallinity and performance indicators.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993116A_ABST
    Figure CN118993116A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing nanocrystalline magnesium oxide from salt lake magnesium salt. The method comprises the following steps: preparing a precursor solution from the magnesium salt; carrying out atomization treatment on the precursor solution so as to form precursor aerosol; and discharging the precursor aerosol at a preset discharge power so as to synthesize the nanocrystalline magnesium oxide. The invention also discloses nanocrystalline magnesium oxide prepared by the method and a device for preparing nanocrystalline magnesium oxide from salt lake magnesium salt. The reactor has the advantages of being simple in structure, capable of running at normal temperature and normal pressure and rapid in starting. Meanwhile, the synthesis process is simple, rapid, green and environment-friendly, and long-term stable operation can be realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of chemical technology, and specifically relates to a method and device for preparing nanocrystalline magnesium oxide from salt lake magnesium salt, and the nanocrystalline magnesium oxide. Background Art

[0002] High-purity nanocrystalline magnesium oxide (MgO) has the advantages of being odorless, non-toxic, cheap, ultra-high melting point, good magnetic conductivity, excellent insulation performance, and chemical stability, and is therefore widely used in the fields of chemical industry, electronics, national defense, medicine, and food. In particular, transparent MgO special ceramics synthesized using high-purity nanocrystalline MgO have the advantages of high melting point, strong thermal conductivity, low density, high insulation, and high infrared transmittance, and have important applications in the fields of spacecraft, rocket and missile infrared windows, high-temperature infrared optical devices, optical filters, and optical detectors. However, the properties of high-purity nanocrystalline MgO (degree of crystallization, grain size, specific surface area, porosity, morphology, and purity) will directly affect the performance of synthetic transparent MgO ceramics, so the controllable synthesis method of high-purity nanocrystalline MgO is extremely critical to the development of the transparent MgO ceramic industry.

[0003] The synthesis of nanocrystalline MgO materials usually adopts methods such as hydrothermal method, sol-gel method, precipitation method and microwave irradiation method. Although the hydrothermal method can adjust the morphology and particle size of the synthesized MgO, the synthesis process is complicated and has a long cycle, and has high requirements for equipment materials. The sol-gel method has the characteristics of simple equipment, controllable and adjustable process, but the production cost is high, the operation is complicated, the production cycle is long, the environmental pollution is large, and the MgO nanoparticles are easy to sinter during the high-temperature crystallization process. The precipitation method is simple to operate and has low requirements for equipment and technology, but it has disadvantages such as long process flow, difficult washing, and a lot of waste liquid. The MgO powder prepared by the precipitation method is usually an amorphous structure and needs to be crystallized by high-temperature calcination. The microwave irradiation method can prepare nanocrystalline MgO powder under normal pressure or high pressure conditions. The product has high purity and does not require post-processing, but the equipment is expensive, the process temperature is very high, and the equipment material requirements are strict. Summary of the invention

[0004] In order to solve the technical problems existing in the above-mentioned prior art, according to an embodiment of the present invention, a method and device for preparing nanocrystalline magnesium oxide from salt lake magnesium salt and nanocrystalline magnesium oxide are provided.

[0005] According to one aspect of an embodiment of the present invention, a method for preparing nanocrystalline magnesium oxide from salt lake magnesium salt includes: preparing a precursor solution using magnesium salt; atomizing the precursor solution to form a precursor aerosol; and discharging the precursor aerosol at a preset discharge power to synthesize nanocrystalline magnesium oxide.

[0006] In an example of the method for preparing nanocrystalline magnesium oxide from salt lake magnesium salt provided in the above aspect, the method of using magnesium salt to prepare a precursor solution includes: mixing the magnesium salt with deionized water to form a precursor solution; or, mixing the magnesium salt with deionized water and ethanol to form a precursor solution.

[0007] In an example of the method for preparing nanocrystalline magnesium oxide from salt lake magnesium salt provided in the above aspect, the method of atomizing the precursor solution includes: passing the precursor solution into an ultrasonic atomization unit, and passing nitrogen into the ultrasonic atomization unit to atomize the precursor solution into a precursor aerosol.

[0008] In an example of the method for preparing nanocrystalline magnesium oxide from salt lake magnesium salt provided in the above aspect, the method of discharging the precursor aerosol at a preset discharge power includes: passing the precursor aerosol into a plasma discharge synthesis unit, and passing air into the plasma discharge synthesis unit, so that the plasma discharge synthesis unit discharges the precursor aerosol at a preset discharge power.

[0009] In one example of the method for preparing nanocrystalline magnesium oxide from salt lake magnesium salt provided in the above aspect, the nitrogen gas has an inlet flow rate of 50 mL / min-500 mL / min.

[0010] In an example of the method for preparing nanocrystalline magnesium oxide from salt lake magnesium salt provided in the above aspect, the preset discharge power is 100W-200W.

[0011] In one example of the method for preparing nanocrystalline magnesium oxide from salt lake magnesium salt provided in the above aspect, the air flow rate is 1 L / min-10 L / min.

[0012] In one example of the method for preparing nanocrystalline magnesium oxide from salt lake magnesium salt provided in the above aspect, the magnesium salt includes at least one of magnesium chloride, magnesium acetate and magnesium sulfate.

[0013] According to another aspect of an embodiment of the present invention, nanocrystalline magnesium oxide is provided, which is prepared by the above method.

[0014] According to another aspect of an embodiment of the present invention, an apparatus for preparing nanocrystalline magnesium oxide from salt lake magnesium salt includes: an ultrasonic atomization unit for receiving a precursor solution prepared from magnesium salt and nitrogen gas to atomize the precursor solution into a precursor aerosol; and a plasma discharge synthesis unit for receiving the precursor aerosol and air to discharge the precursor aerosol to synthesize nanocrystalline magnesium oxide.

[0015] Beneficial effects: According to the method and device for preparing nanocrystalline magnesium oxide from salt lake magnesium salt and nanocrystalline magnesium oxide of the embodiments of the present invention, the reactor has a simple structure, can be operated at normal temperature and pressure, and can be started quickly. At the same time, the synthesis process is simple, fast, green and environmentally friendly, and can be operated stably for a long time. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] The above and other aspects, features and advantages of the embodiments of the present invention will become more apparent through the following description in conjunction with the accompanying drawings, in which:

[0017] Figure 1 is a flow chart of a method for preparing nanocrystalline magnesium oxide from salt lake magnesium salt according to an embodiment of the present invention;

[0018] Figure 2 is a schematic structural diagram of an apparatus for preparing nanocrystalline magnesium oxide from salt lake magnesium salt according to an embodiment of the present invention;

[0019] Figure 3 is an XRD diagram of nanocrystalline magnesium oxide prepared according to the first embodiment of the present invention;

[0020] Figure 4 is an XRD diagram of nanocrystalline magnesium oxide prepared according to the second embodiment of the present invention;

[0021] Figure 5 is an XRD diagram of nanocrystalline magnesium oxide prepared according to the third embodiment of the present invention;

[0022] Figure 6 is an XRD diagram of nanocrystalline magnesium oxide prepared according to the fourth embodiment of the present invention;

[0023] Figure 7 is an XRD diagram of nanocrystalline magnesium oxide prepared according to the fifth embodiment of the present invention;

[0024] Figure 8 is an XRD diagram of nanocrystalline magnesium oxide prepared according to Embodiment 6 of the present invention;

[0025] Fig. 9 3 is an XRD diagram of nanocrystalline magnesium oxide prepared according to Embodiment 7 of the present invention. DETAILED DESCRIPTION

[0026] Hereinafter, specific embodiments of the present invention will be described in detail with reference to the accompanying drawings. However, the present invention may be implemented in many different forms, and the present invention should not be construed as being limited to the specific embodiments set forth herein. On the contrary, these embodiments are provided to explain the principles of the present invention and their practical applications, so that other persons skilled in the art can understand the various embodiments of the present invention and various modifications suitable for specific intended applications.

[0027] As used herein, the term "including" and its variations represent open terms, meaning "including but not limited to". The terms "based on", "according to", etc. mean "based at least in part on", "based at least in part on". The terms "one embodiment" and "an embodiment" mean "at least one embodiment". The term "another embodiment" means "at least one other embodiment". The terms "first", "second", etc. may refer to different or the same objects. Other definitions may be included below, whether explicit or implicit. Unless the context clearly indicates otherwise, the definition of a term is consistent throughout the specification.

[0028] Figure 1 The present invention is a flowchart of a method for preparing nanocrystalline magnesium oxide from salt lake magnesium salt according to an embodiment of the present invention.

[0029] Reference Figure 1 According to an embodiment of the present invention, the method for preparing nanocrystalline magnesium oxide from salt lake magnesium salt comprises:

[0030] Step S110: preparing a precursor solution using magnesium salt;

[0031] Step S120: atomizing the precursor solution to form a precursor aerosol;

[0032] Step S130: discharging the precursor aerosol at a preset discharge power to synthesize nanocrystalline magnesium oxide.

[0033] Furthermore, the method of preparing a precursor solution using magnesium salt includes: mixing the magnesium salt with deionized water to form a precursor solution; or, mixing the magnesium salt with deionized water and ethanol to form a precursor solution.

[0034] Furthermore, the method of atomizing the precursor solution includes: passing the precursor solution into an ultrasonic atomization unit, and passing nitrogen into the ultrasonic atomization unit, so as to atomize the precursor solution into a precursor aerosol.

[0035] Furthermore, the method of discharging the precursor aerosol at a preset discharge power includes: passing the precursor aerosol into a plasma discharge synthesis unit, and passing air into the plasma discharge synthesis unit, so that the plasma discharge synthesis unit discharges the precursor aerosol at a preset discharge power.

[0036] Furthermore, the nitrogen gas has an inlet flow rate of 50 mL / min-500 mL / min.

[0037] Furthermore, the preset discharge power is 100W-200W.

[0038] Furthermore, the air flow rate is 1L / min-10L / min.

[0039] Furthermore, the magnesium salt includes at least one of magnesium chloride, magnesium acetate and magnesium sulfate.

[0040] Figure 2 It is a schematic structural diagram of an apparatus for preparing nanocrystalline magnesium oxide from salt lake magnesium salt according to an embodiment of the present invention.

[0041] Reference Figure 2 The device for preparing nanocrystalline magnesium oxide from salt lake magnesium salt according to an embodiment of the present invention includes: an ultrasonic atomization unit 100, a plasma discharge synthesis unit 200, a collection unit 300 and an exhaust gas treatment unit 400.

[0042] The ultrasonic atomization unit 100 is used to receive a precursor solution prepared by magnesium salt and nitrogen gas to atomize the precursor solution into a precursor aerosol.

[0043] The plasma discharge synthesis unit 200 is used to receive the precursor aerosol and air introduced, so as to discharge the precursor aerosol, thereby synthesizing nanocrystalline magnesium oxide. That is to say, the plasma discharge synthesis unit 200 is a reactor for synthesizing nanocrystalline magnesium oxide. Specifically, the plasma discharge synthesis unit 200 includes an inlet 210, an outlet 220 arranged opposite to the inlet 210, and a high-voltage electrode 230 and a ground electrode 240 respectively arranged on both sides of the precursor aerosol flow channel formed by the inlet 210 and the outlet 220. The inlet 210 is used to receive the precursor aerosol and air introduced, and a discharge plasma is generated by breaking down between the high-voltage electrode 230 and the ground electrode 240, and the precursor aerosol entering the discharge area is oxidized, thereby synthesizing nanocrystalline magnesium oxide. The outlet 220 is used to collect the synthesized nanocrystalline magnesium oxide in the collection unit 300. The tail gas treatment unit 400 is used to absorb and treat the tail gas using alkaline solution (such as but not limited to sodium hydroxide) to reduce pollution to the environment.

[0044] Furthermore, the high voltage electrode 230 and the ground electrode 240 are driven by an alternating current power source.

[0045] The following is a detailed description of the method for preparing nanocrystalline magnesium oxide according to an embodiment of the present invention.

[0046] <Implementation Method 1>

[0047] Weigh 20g of magnesium acetate and add 60g of deionized water to prepare a precursor solution. Set the plasma discharge power to 100W, the air gas flow rate to 3L / min, the nitrogen carrier gas flow rate to 200mL / min, and the AC frequency to 40kHz. The grain size of the synthesized nanocrystalline magnesium oxide is 8.0nm, the particle size of the synthesized nanocrystalline magnesium oxide is 11nm, and the specific surface area of ​​the synthesized nanocrystalline magnesium oxide is 83m 2 / g, the pore size of the synthesized nanocrystalline magnesium oxide is 13nm, and the pore volume of the synthesized nanocrystalline magnesium oxide is 0.28cm 3 / g.

[0048] Figure 3 : is an XRD diagram of nanocrystalline magnesium oxide prepared according to the first embodiment of the present invention. Figure 3 The XRD pattern shows the typical diffraction characteristics of nanocrystalline MgO, where the characteristic diffraction peak at 2θ of 42.9 degrees corresponds to the (200) crystal plane of MgO, and the characteristic diffraction peak at 2θ of 62.3 degrees corresponds to the (220) crystal plane of MgO. The peaks are sharp and have high intensity, indicating that the MgO nanopowder has good crystallinity.

[0049] <Implementation Method 2>

[0050] Weigh 20g of magnesium acetate, add 40g of deionized water and 20g of ethanol to prepare a precursor solution. The plasma discharge power is 100W, the air gas flow rate is 3L / min, the nitrogen carrier gas flow rate is 200mL / min, and the AC frequency is 40kHz. The grain size of the synthesized nanocrystalline magnesium oxide is 13.0nm, the particle size of the synthesized nanocrystalline magnesium oxide is 11.9nm, and the specific surface area of ​​the synthesized nanocrystalline magnesium oxide is 128m 2 / g, the pore size of the synthesized nanocrystalline magnesium oxide is 14.7nm, and the pore volume of the synthesized nanocrystalline magnesium oxide is 0.442cm 3 / g.

[0051] Figure 4 1 is an XRD diagram of nanocrystalline magnesium oxide prepared according to the second embodiment of the present invention.

[0052] <Implementation Method 3>

[0053] Weigh 20g of magnesium acetate, add 40g of deionized water and 20g of ethanol to prepare a precursor solution. The plasma discharge power is 140W, the air gas flow rate is 6L / min, the nitrogen carrier gas flow rate is 200mL / min, and the AC frequency is 40kHz. The grain size of the synthesized nanocrystalline magnesium oxide is 10.0nm, the particle size of the synthesized nanocrystalline magnesium oxide is 7.40nm, and the specific surface area of ​​the synthesized nanocrystalline magnesium oxide is 140m 2 / g, the pore size of the synthesized nanocrystalline magnesium oxide is 16.4nm, and the pore volume of the synthesized nanocrystalline magnesium oxide is 0.490cm 3 / g.

[0054] Figure 5 1 is an XRD diagram of nanocrystalline magnesium oxide prepared according to the third embodiment of the present invention.

[0055] <Implementation Method 4>

[0056] Weigh 20g of magnesium chloride and add 60g of deionized water to prepare a precursor solution. The plasma discharge power is 100W, the air gas flow rate is 3L / min, the nitrogen carrier gas flow rate is 200mL / min, and the AC frequency is 40kHz. The grain size of the synthesized nanocrystalline magnesium oxide is 14nm, the particle size of the synthesized nanocrystalline magnesium oxide is 24nm, and the specific surface area of ​​the synthesized nanocrystalline magnesium oxide is 49.0907m 2 / g, the pore size of the synthesized nanocrystalline magnesium oxide is 17.518nm, and the pore volume of the synthesized nanocrystalline magnesium oxide is 0.25283cm 3 / g.

[0057] Figure 6 1 is an XRD diagram of nanocrystalline magnesium oxide prepared according to the fourth embodiment of the present invention.

[0058] <Implementation Method Five>

[0059] Weigh 20g of magnesium chloride, add 40g of deionized water and 20g of ethanol to prepare a precursor solution. The plasma discharge power is 100W, the air gas flow rate is 3L / min, the nitrogen carrier gas flow rate is 200mL / min, and the AC frequency is 40kHz. The grain size of the synthesized nanocrystalline magnesium oxide is 17.0nm, the particle size of the synthesized nanocrystalline magnesium oxide is 10.9nm, and the specific surface area of ​​the synthesized nanocrystalline magnesium oxide is 41.5m 2 / g, the pore size of the synthesized nanocrystalline magnesium oxide is 15.9nm, and the pore volume of the synthesized nanocrystalline magnesium oxide is 0.157cm 3 / g.

[0060] Figure 7 1 is an XRD diagram of nanocrystalline magnesium oxide prepared according to the fifth embodiment of the present invention.

[0061] <Implementation Method Six>

[0062] Weigh 20g of magnesium acetate, add 40g of deionized water and 20g of ethanol to prepare a precursor solution. The plasma discharge power is 140W, the air gas flow rate is 6L / min, the nitrogen carrier gas flow rate is 200mL / min, and the AC frequency is 40kHz. The grain size of the synthesized nanocrystalline magnesium oxide is 16.0nm, the particle size of the synthesized nanocrystalline magnesium oxide is 35.5nm, and the specific surface area of ​​the synthesized nanocrystalline magnesium oxide is 89.2m 2 / g, the pore size of the synthesized nanocrystalline magnesium oxide is 18.4nm, and the pore volume of the synthesized nanocrystalline magnesium oxide is 0.112cm 3 / g.

[0063] Figure 8 1 is an XRD diagram of nanocrystalline magnesium oxide prepared according to Embodiment 6 of the present invention.

[0064] <Implementation Method Seven>

[0065] Weigh 20g of magnesium sulfate, add 40g of deionized water and 20g of ethanol to prepare a precursor solution. The plasma discharge power is 100W, the air gas flow rate is 3L / min, the nitrogen carrier gas flow rate is 200mL / min, and the AC frequency is 40kHz. The grain size of the synthesized nanocrystalline magnesium oxide is 18.0nm, the particle size of the synthesized nanocrystalline magnesium oxide is 13nm, and the specific surface area of ​​the synthesized nanocrystalline magnesium oxide is 91m 2 / g, the pore size of the synthesized nanocrystalline magnesium oxide is 18nm, and the pore volume of the synthesized nanocrystalline magnesium oxide is 0.36cm 3 / g.

[0066] Fig. 9 3 is an XRD diagram of nanocrystalline magnesium oxide prepared according to Embodiment 7 of the present invention.

[0067] In summary, the method and device for preparing nanocrystalline magnesium oxide from salt lake magnesium salt and nanocrystalline magnesium oxide according to the embodiments of the present invention have a simple reactor structure, can be operated at room temperature and pressure, and can be started quickly. At the same time, the synthesis process is simple, fast, green and environmentally friendly, and can be operated stably for a long time.

[0068] The terms "exemplary," "example," and the like used throughout this specification mean "used as an example, instance, or illustration" and do not mean "preferred" or "advantageous" over other embodiments. The detailed description includes specific details for the purpose of providing an understanding of the described techniques. However, these techniques can be implemented without these specific details. In some instances, in order to avoid obscuring the concepts of the described embodiments, well-known structures and devices are shown in block diagram form.

[0069] The optional implementation modes of the embodiments of the present invention are described in detail above in conjunction with the accompanying drawings. However, the embodiments of the present invention are not limited to the specific details in the above implementation modes. Within the technical concept of the embodiments of the present invention, various simple modifications can be made to the technical solutions of the embodiments of the present invention, and these simple modifications all belong to the protection scope of the embodiments of the present invention.

[0070] The above description of the contents of this specification is provided to enable any person of ordinary skill in the art to implement or use the contents of this specification. Various modifications to the contents of this specification will be apparent to those of ordinary skill in the art, and the general principles defined herein may be applied to other variations without departing from the scope of protection of the contents of this specification. Therefore, the contents of this specification are not limited to the examples and designs described herein, but are consistent with the widest range of principles and novel features disclosed herein.

Claims

1. A method for preparing nanocrystalline magnesium oxide from salt lake magnesium salt, characterized in that: The method comprises: A precursor solution is prepared using magnesium salt; Atomizing the precursor solution to form a precursor aerosol; The precursor aerosol is discharged at a preset discharge power to synthesize nanocrystalline magnesium oxide.

2. The method according to claim 1, characterized in that The method of using magnesium salt to prepare a precursor solution includes: mixing the magnesium salt with deionized water to form a precursor solution; or mixing the magnesium salt with deionized water and ethanol to form a precursor solution.

3. The method according to claim 1, characterized in that The method for atomizing the precursor solution comprises: passing the precursor solution into an ultrasonic atomization unit, and passing nitrogen into the ultrasonic atomization unit, so as to atomize the precursor solution into a precursor aerosol.

4. The method according to claim 1, characterized in that: The method for discharging the precursor aerosol with a preset discharge power includes: passing the precursor aerosol into a plasma discharge synthesis unit, and passing air into the plasma discharge synthesis unit, so that the plasma discharge synthesis unit discharges the precursor aerosol with the preset discharge power.

5. The method according to claim 3, characterized in that: The nitrogen gas flow rate is 50 mL / min-500 mL / min.

6. The method according to claim 4, characterized in that The preset discharge power is 100W-200W.

7. The method according to claim 4, characterized in that The air flow rate is 1L / min-10L / min.

8. The method according to any one of claims 1 to 7, characterized in that: The magnesium salt includes at least one of magnesium chloride, magnesium acetate and magnesium sulfate.

9. A nanocrystalline magnesium oxide, characterized in that: The nanocrystalline magnesium oxide is prepared by the method according to any one of claims 1 to 8.

10. A device for preparing nanocrystalline magnesium oxide from salt lake magnesium salt, characterized in that: The device comprises: An ultrasonic atomization unit, used for receiving a precursor solution prepared by magnesium salt and nitrogen gas, so as to atomize the precursor solution into a precursor aerosol; The plasma discharge synthesis unit is used to receive the precursor aerosol and air to discharge the precursor aerosol, thereby synthesizing nanocrystalline magnesium oxide.