Preparation method of magnesium oxide for low-temperature high-magnetic-induction oriented silicon steel

By preparing and stabilizing magnesium oxide to control its activity index, the problem of excessive magnesium oxide activity leading to excessive formation of the bottom layer is solved, and the excellent bottom layer and magnetic properties of low-temperature and high magnetic inductance oriented silicon steel are achieved.

CN118993117AInactive Publication Date: 2024-11-22HEBEI MEITAI MAGNESIUM MATERIAL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411282663.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing magnesium oxide activity is too high, resulting in the formation of the magnesium silicate base layer too fast, affecting the magnetic properties and surface properties of low-temperature and high-magnetic induction oriented silicon steel.

Method used

A method for preparing magnesium oxide for low-temperature high magnetic induction oriented silicon steel, including preparing magnesium oxide crystal precursor, preparing nanomagnesium oxide, stabilizing magnesium oxide and assembling stabilize magnesium oxide and nanomagnesium oxide, and controlling magnesium oxide Activity indicators CAA30 and CAA70 ensure the formation time of the bottom layer and the release of gas phase N.

Benefits of technology

It realizes rapid reaction at low temperature to form an excellent magnesium silicate bottom layer, avoids crystal leakage, improves magnetic and surface properties, and ensures full release of gas phase N.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993117A_ABST
    Figure CN118993117A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of magnesium oxide for low-temperature high-magnetic-induction oriented silicon steel, and belongs to the technical field of magnesium oxide preparation. Comprising the following steps: preparing a magnesium oxide crystal precursor; preparing nano magnesium oxide; stabilizing the magnesium oxide; and assembling the stabilized magnesium oxide and the nano magnesium oxide. Nano magnesium oxide is prepared to serve as a main body of magnesium oxide for low-temperature high-magnetic-induction oriented silicon steel, the specific surface area of the magnesium oxide is greatly increased due to the nanoscale size, so that the surface activity and reactivity of the material are enhanced, and after the surface of the oriented silicon steel is coated with the magnesium oxide, due to the high specific surface area of the nano magnesium oxide, the specific surface area of the magnesium oxide is increased; the magnesium oxide can be compactly arranged on the surface of the oriented silicon steel, and granular oxide gathers on the surface of the oriented silicon steel along with temperature rise to form a compact magnesium silicate layer, so that the bottom layer of the oriented silicon steel is covered with the magnesium oxide, and crystal leakage is prevented.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of magnesium oxide preparation, and in particular to a method for preparing magnesium oxide for low-temperature and high-magnetic-induction oriented silicon steel. Background Art

[0002] Oriented silicon steel is widely used as a magnetic core material. In recent years, the social demand for energy conservation and resource saving has become increasingly urgent, and the demand for reducing the iron loss of oriented silicon steel and improving the magnetization characteristics has also become strong. Oriented silicon steel should be coated with an annealing separator before high-temperature annealing, and then rolled into a coil after drying and sent to a high-temperature annealing furnace for annealing. The role of the magnesium oxide annealing separator is to prevent the steel plate from sticking, promote desulfurization and denitrification reactions during high-temperature purification annealing, and generate a magnesium silicate bottom layer on the surface of the steel plate. The magnetic properties and surface properties of oriented silicon steel are closely related to the magnesium silicate bottom layer, so the quality of the magnesium silicate bottom layer is extremely important.

[0003] The prior art, such as the method disclosed in patent CN114573009A, which uses dolomite and bischofite as raw materials to prepare magnesium oxide for silicon steel, has a high eutectic shape of the prepared magnesium oxide, which easily causes the bottom layer to form too quickly, and is not conducive to the release of gas phase N in low-temperature and high-magnetic induction oriented silicon steel. Therefore, the present invention provides a method for preparing magnesium oxide for low-temperature and high-magnetic induction oriented silicon steel to solve the above technical problems. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a method for preparing magnesium oxide for low-temperature high-magnetic induction oriented silicon steel to solve the problem that the existing magnesium oxide is too active and the bottom layer is formed too quickly.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] A method for preparing magnesium oxide for low-temperature and high-magnetic-induction oriented silicon steel comprises the following steps:

[0007] S1: Preparation of magnesium oxide crystal precursor

[0008] Weighing MgCl2·6H2O and AlCl3·6H2O and ultrasonically dissolving them in deionized water, and then weighing urea and ultrasonically dissolving them in deionized water to obtain a mixed solution, transferring the mixed solution to a polytetrafluoroethylene reactor for reaction, and then naturally cooling it to room temperature to obtain a suspension, centrifuging the suspension, and then washing the precipitate with deionized water, drying the washed precipitate, and then taking it out and grinding it to obtain a magnesium oxide crystal precursor;

[0009] S2: Preparation of Nano-MgO

[0010] The magnesium oxide crystal precursor is evenly spread on the bottom of the magnetic boat, and the magnetic boat is placed in a muffle furnace for calcination to obtain magnesium oxide powder in the magnetic boat. After the magnetic boat is taken out, the magnesium oxide powder is allowed to stand and cool to room temperature, and then ultrasonically dispersed to obtain nano magnesium oxide.

[0011] S3: Stabilization of magnesium oxide

[0012] The magnesium oxide powder, sodium nitrate and sodium carbonate are crushed and mixed to obtain a mixed powder, the mixed powder is added to an ethanol dispersant for impregnation, and then vacuum dried to obtain a composite magnesium oxide powder, and then the composite magnesium oxide powder is added to polyvinyl alcohol, the temperature is increased, and ammonia water is added dropwise to adjust the pH, and then magnetic stirring is performed, and centrifugal drying is performed to obtain stabilized magnesium oxide;

[0013] S4: Assembling stabilized MgO and nano-MgO

[0014] Deionized water is added to the stabilized magnesium oxide to form a wet sample, and the wet sample is pressed into thin slices, dried, and the dried thin slices are broken to obtain stabilized magnesium oxide particles. Nano-magnesium oxide is mixed with the stabilized magnesium oxide particles to obtain magnesium oxide for low-temperature and high magnetic induction oriented silicon steel.

[0015] Optionally, step S1 of preparing a magnesium oxide crystal precursor comprises the following steps:

[0016] S1.1: Weigh 10-12 parts by mass of MgCl2·6H2O and 5-6 parts by mass of AlCl3·6H2O and dissolve them in deionized water by ultrasonic, and then weigh 20-22 parts by mass of urea and dissolve them in deionized water by ultrasonic to obtain a mixed solution;

[0017] S1.2: The mixed solution is transferred to a polytetrafluoroethylene reactor, reacted at 180-200°C for 30-32 hours, and then naturally cooled to room temperature to obtain a suspension;

[0018] S1.3: Centrifuge the suspension at 3900-4000 r / min for 3-5 min, and then wash the precipitate with deionized water until the washing solution is neutral;

[0019] S1.4: The washed precipitate is placed in an oven at 70-80°C and dried for 20-24 hours, then taken out and ground through a 120-mesh sieve to obtain a magnesium oxide crystal precursor.

[0020] Optionally, in step S1.1, the Mg2+ concentration of MgCl2·6H2O is 0.2 mol / L, and the Al3+ concentration of AlCl3·6H2O is 0.1 mol / L.

[0021] Optionally, the urea concentration in step S1.1 is 2 mol / L.

[0022] Optionally, step S2 of preparing nano magnesium oxide comprises the following steps:

[0023] S2.1: Spread the magnesium oxide crystal precursor evenly on the bottom of the magnetic boat with a thickness of 5-10 mm, place the magnetic boat in a muffle furnace, and calcine at a temperature of 550-580°C for 3-3.2 h with a heating rate of 10°C / min and an initial temperature of 20°C to obtain magnesium oxide powder in the magnetic boat;

[0024] S2.2: After taking out the magnetic boat, let the magnesium oxide powder stand for 10-20 minutes to cool to room temperature, and then ultrasonically disperse it for 20-30 minutes to obtain nano magnesium oxide.

[0025] S3: Stabilization of magnesium oxide

[0026] Optionally, step S3 stabilizes the magnesium oxide, comprising the following steps:

[0027] S3.1: crushing magnesium oxide powder, sodium nitrate and sodium carbonate and mixing them to obtain a mixed powder, adding the mixed powder into an ethanol dispersant, immersing at 75-80° C. for 10-12 hours, and then vacuum drying at 100-120° C. for 24-26 hours to obtain composite magnesium oxide powder;

[0028] S3.2: Add the composite magnesium oxide powder to 15wt% polyvinyl alcohol, raise the temperature to 50-60°C, add ammonia water to adjust the pH to 10, and then stir magnetically at a speed of 500-600r / min for 15-30min, centrifuge and dry to obtain stabilized magnesium oxide.

[0029] Optionally, the mass ratio of magnesium oxide, sodium nitrate and sodium carbonate is 30:2:1.

[0030] Optionally, the solid-liquid ratio of the mixed powder and the ethanol dispersant is 1:3.

[0031] Optionally, the material-liquid ratio of the composite magnesium oxide powder and polyvinyl alcohol is 1:5.

[0032] Optionally, step S4 assembling stabilized magnesium oxide and nano magnesium oxide comprises the following steps:

[0033] S4.1: Add 10% of the system volume of deionized water to the stabilized magnesium oxide to form a wet sample, press the wet sample into flakes, dry at 50-60° C., and crush the dried flakes into 1-4 mm particles to obtain stabilized magnesium oxide particles;

[0034] S4.2: Mix nano magnesium oxide and stabilized magnesium oxide particles in a mass ratio of 2:1 to obtain magnesium oxide for low-temperature and high magnetic induction oriented silicon steel.

[0035] In the present invention, CAA30 and CAA70 are used as activity indicators of magnesium oxide. 30 and 70 represent the time (seconds) required for the reaction of magnesium oxide and citric acid to reach 30% and 70%, respectively. The shorter the time, the higher the activity.

[0036] CAA30 is used to evaluate the activity index of magnesium oxide for low-temperature and high magnetic induction oriented silicon steel, and CAA30 is controlled at 60-80s.

[0037] CAA70 is used to evaluate the activity index of magnesium oxide for low-temperature and high magnetic induction oriented silicon steel, and CAA70 is controlled at 160-220s.

[0038] The present invention simultaneously controls CAA30 and CAA70, so that on the one hand, magnesium oxide has high activity and can react quickly at low temperature to form a magnesium silicate bottom layer. On the other hand, by controlling the low activity index, the formation time of the bottom layer can be controlled, thereby ensuring that the gas phase N in the low-temperature high magnetic induction oriented silicon steel can be fully released, and finally obtaining the low-temperature high magnetic induction oriented silicon steel with excellent bottom layer and magnetic properties.

[0039] The obtained magnesium oxide has a purity of 98.5-99.5%, uniform particles, low hydration rate, CAA30 of 60-80 seconds, and CAA70 of 160-220 seconds.

[0040] The prepared magnesium oxide for low temperature high magnetic induction oriented silicon steel was mixed with water in a ratio of 1:8, and 2% TiO2 was added based on the mass percentage of MgO, and stirred evenly. 2 The coating amount is applied on the surface of low-temperature and high-magnetic induction oriented silicon steel (the oriented silicon steel is composed of the following components in weight percentage: C0.02%, Si 3.5%, Mn 0.006%, Al0.03%, S 0.005%, P 0.015%, N 0.007%, and the rest is Fe and inevitable impurities), dried, and high-temperature annealed in a ring furnace to form an excellent bottom layer on the surface of the low-temperature and high-magnetic induction oriented silicon steel.

[0041] Compared with the prior art, the present invention has at least the following beneficial effects:

[0042] In the above scheme, nano-magnesium oxide is prepared as the main body of magnesium oxide for low-temperature and high magnetic induction oriented silicon steel. The nano-scale size greatly increases its specific surface area, thereby enhancing the surface activity and reactivity of the material. After the magnesium oxide is coated on the surface of the oriented silicon steel, due to the high specific surface area of ​​the nano-magnesium oxide, the magnesium oxide can be densely arranged on the surface of the oriented silicon steel. As the temperature rises, the granular oxide gathers to the surface of the oriented silicon steel to form a dense magnesium silicate layer, thereby covering the bottom layer of the oriented silicon steel and preventing crystal leakage.

[0043] The present invention also performs a stabilization treatment on the magnesium oxide. Since the oriented silicon steel will undergo a denitrification reaction during the annealing process, and the magnesium oxide is also an adsorbent, and when the magnesium oxide has a large specific surface area and high activity, when the oriented silicon steel is denitrified, the magnesium oxide is easy to adsorb nitrogen and adhere to the surface, thereby destroying the dense arrangement between the magnesium oxides, resulting in invisible crystal leakage or point-like crystal leakage defects when the magnesium silicate layer is formed. Therefore, by stabilizing the magnesium oxide, sodium nitrate and sodium carbonate are compounded on the surface of the magnesium oxide, thereby reducing the defects in the outer layer of the magnesium oxide crystal structure, so that the adsorption capacity of the magnesium oxide for nitrogen decreases. In addition, due to the surface-stable non-notch structure formed after the sodium nitrate and sodium carbonate are compounded with the magnesium oxide, uneven arrangement and crystal leakage will not occur when the magnesium silicate layer is formed. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] The accompanying drawings, which are incorporated herein and constitute a part of the specification, illustrate embodiments of the invention and, together with the description, further serve to explain the principles of the invention and to enable those skilled in the relevant art to make and use the invention.

[0045] Figure 1 This is a flow chart of a method for preparing magnesium oxide for low-temperature and high magnetic induction oriented silicon steel adopted in an embodiment of the present invention. DETAILED DESCRIPTION

[0046] The AA provided by the present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. At the same time, it is explained here that in order to make the embodiments more detailed, the following embodiments are the best and preferred embodiments, and those skilled in the art may also adopt other alternatives to implement some known technologies; and the accompanying drawings are only for a more specific description of the embodiments, and are not intended to specifically limit the present invention.

[0047] Embodiment 1:

[0048] A method for preparing magnesium oxide for low-temperature high magnetic induction oriented silicon steel, such as Figure 1 As shown, the following steps are included:

[0049] S1: Preparation of magnesium oxide crystal precursor

[0050] S1.1: Weigh 10 parts by mass of MgCl2·6H2O and 5 parts by mass of AlCl3·6H2O and dissolve them in deionized water by ultrasonic. 2+ The concentration is 0.2mol / L, AlCl3·6H2O 3+ The concentration is 0.1 mol / L, and 20 parts by mass of 2 mol / L urea are weighed and ultrasonically dissolved in 30 mL of deionized water to obtain a mixed solution;

[0051] S1.2: The mixed solution was transferred to a polytetrafluoroethylene reactor, reacted at 180°C for 30 hours, and then naturally cooled to room temperature to obtain a suspension;

[0052] S1.3: Centrifuge the suspension at 3900 r / min for 3 min, and then wash the precipitate with deionized water until the washing solution is neutral;

[0053] S1.4: The washed precipitate is placed in an oven at 80°C and dried for 24 hours, then taken out and ground through a 120-mesh sieve to obtain a magnesium oxide crystal precursor.

[0054] S2: Preparation of Nano-MgO

[0055] S2.1: Spread the magnesium oxide crystal precursor evenly on the bottom of the magnetic boat with a thickness of 5 mm, place the magnetic boat in a muffle furnace, and bake at 550°C for 3 hours with a heating rate of 10°C / min and an initial temperature of 20°C to obtain magnesium oxide powder in the magnetic boat;

[0056] S2.2: After taking out the magnetic boat, let the magnesium oxide powder stand for 10 minutes to cool to room temperature, and then ultrasonically disperse it for 30 minutes to obtain nano magnesium oxide of 10-40 nm.

[0057] S3: Stabilization of magnesium oxide

[0058] S3.1: crushing magnesium oxide powder, sodium nitrate and sodium carbonate and mixing them, the mass ratio of magnesium oxide, sodium nitrate and sodium carbonate is 30:2:1, and obtaining a mixed powder; adding the mixed powder into an ethanol dispersant, the material-liquid ratio of the mixed powder to the ethanol dispersant is 1:3; immersing at 80°C for 12h, and then vacuum drying at 100°C for 24h to obtain a composite magnesium oxide powder;

[0059] S3.2: Add the composite magnesium oxide powder into 15wt% polyvinyl alcohol, with the material-liquid ratio of composite magnesium oxide powder to polyvinyl alcohol being 1:5, raise the temperature to 50°C, add ammonia water to adjust the pH to 10, and then stir magnetically at a speed of 500r / min for 30min, centrifuge and dry to obtain stabilized magnesium oxide.

[0060] S4: Assembling stabilized MgO and nano-MgO

[0061] S4.1: Add 10% of the system volume of deionized water to the stabilized magnesium oxide to form a wet sample, press the wet sample into flakes, dry at 50°C, and crush the dried flakes into 1-4 mm particles to obtain stabilized magnesium oxide particles;

[0062] S4.2: Mix nano magnesium oxide and stabilized magnesium oxide particles in a mass ratio of 2:1 to obtain magnesium oxide for low-temperature and high magnetic induction oriented silicon steel.

[0063] Embodiment 2:

[0064] A method for preparing magnesium oxide for low-temperature high magnetic induction oriented silicon steel, such as Figure 1 As shown, the following steps are included:

[0065] S1: Preparation of magnesium oxide crystal precursor

[0066] S1.1: Weigh 12 parts by mass of MgCl2·6H2O and 6 parts by mass of AlCl3·6H2O and dissolve them in deionized water by ultrasonic. 2+ The concentration is 0.2mol / L, AlCl3·6H2O 3+ The concentration is 0.1 mol / L, and 22 parts by mass of 2 mol / L urea is ultrasonically dissolved in deionized water to obtain a mixed solution;

[0067] S1.2: The mixed solution was transferred to a polytetrafluoroethylene reactor, reacted at 180°C for 30 hours, and then naturally cooled to room temperature to obtain a suspension;

[0068] S1.3: Centrifuge the suspension at 3900 r / min for 3 min, and then wash the precipitate with deionized water until the washing solution is neutral;

[0069] S1.4: The washed precipitate is placed in an oven at 80°C and dried for 24 hours, then taken out and ground through a 120-mesh sieve to obtain a magnesium oxide crystal precursor.

[0070] S2: Preparation of Nano-MgO

[0071] S2.1: Spread the magnesium oxide crystal precursor evenly on the bottom of the magnetic boat with a thickness of 5 mm, place the magnetic boat in a muffle furnace, and bake at 550°C for 3 hours with a heating rate of 10°C / min and an initial temperature of 20°C to obtain magnesium oxide powder in the magnetic boat;

[0072] S2.2: After taking out the magnetic boat, let the magnesium oxide powder stand for 10 minutes to cool to room temperature, and then ultrasonically disperse it for 30 minutes to obtain nano magnesium oxide of 10-40 nm.

[0073] S3: Stabilization of magnesium oxide

[0074] S3.1: crushing magnesium oxide powder, sodium nitrate and sodium carbonate and mixing them, the mass ratio of magnesium oxide, sodium nitrate and sodium carbonate is 30:2:1, and obtaining a mixed powder; adding the mixed powder into an ethanol dispersant, the material-liquid ratio of the mixed powder to the ethanol dispersant is 1:3; immersing at 80°C for 12h, and then vacuum drying at 100°C for 24h to obtain a composite magnesium oxide powder;

[0075] S3.2: Add the composite magnesium oxide powder into 15wt% polyvinyl alcohol, with the material-liquid ratio of composite magnesium oxide powder to polyvinyl alcohol being 1:5, raise the temperature to 50°C, add ammonia water to adjust the pH to 10, and then stir magnetically at a speed of 500r / min for 30min, centrifuge and dry to obtain stabilized magnesium oxide.

[0076] S4: Assembling stabilized MgO and nano-MgO

[0077] S4.1: Add 10% of the system volume of deionized water to the stabilized magnesium oxide to form a wet sample, press the wet sample into flakes, dry at 50°C, and crush the dried flakes into 1-4 mm particles to obtain stabilized magnesium oxide particles;

[0078] S4.2: Mix nano magnesium oxide and stabilized magnesium oxide particles in a mass ratio of 2:1 to obtain magnesium oxide for low-temperature and high magnetic induction oriented silicon steel.

[0079] Embodiment 3:

[0080] A method for preparing magnesium oxide for low-temperature high magnetic induction oriented silicon steel, such as Figure 1 As shown, the following steps are included:

[0081] S1: Preparation of magnesium oxide crystal precursor

[0082] S1.1: Weigh 10 parts by mass of MgCl2·6H2O and 5 parts by mass of AlCl3·6H2O and dissolve them in deionized water by ultrasonic. 2+ The concentration is 0.2mol / L, AlCl3·6H2O 3+ The concentration is 0.1 mol / L, and 20 parts by mass of 2 mol / L urea is ultrasonically dissolved in deionized water to obtain a mixed solution;

[0083] S1.2: The mixed solution was transferred to a polytetrafluoroethylene reactor, reacted at 200°C for 32 hours, and then naturally cooled to room temperature to obtain a suspension;

[0084] S1.3: Centrifuge the suspension at 4000 r / min for 5 min, and then wash the precipitate with deionized water until the washing solution is neutral;

[0085] S1.4: The washed precipitate is placed in a 70°C oven and dried for 20 hours, then taken out and ground through a 120-mesh sieve to obtain a magnesium oxide crystal precursor.

[0086] S2: Preparation of Nano-MgO

[0087] S2.1: Spread the magnesium oxide crystal precursor evenly on the bottom of the magnetic boat with a thickness of 5 mm, place the magnetic boat in a muffle furnace, and calcine at 580°C for 3.2 h with a heating rate of 10°C / min and an initial temperature of 20°C to obtain magnesium oxide powder in the magnetic boat;

[0088] S2.2: After taking out the magnetic boat, let the magnesium oxide powder stand for 20 minutes to cool to room temperature, and then ultrasonically disperse it for 20 minutes to obtain nano magnesium oxide of 10-40 nm.

[0089] S3: Stabilization of magnesium oxide

[0090] S3.1: Crush magnesium oxide powder, sodium nitrate and sodium carbonate and mix them, the mass ratio of magnesium oxide, sodium nitrate and sodium carbonate is 30:2:1, and obtain mixed powder; add the mixed powder into ethanol dispersant, the material-liquid ratio of the mixed powder and ethanol dispersant is 1:3; immerse at 80°C for 10 hours, and then vacuum dry at 120°C for 26 hours to obtain composite magnesium oxide powder;

[0091] S3.2: Add the composite magnesium oxide powder into 15wt% polyvinyl alcohol, with the material-liquid ratio of composite magnesium oxide powder to polyvinyl alcohol being 1:5, raise the temperature to 60°C, add ammonia water dropwise to adjust the pH to 10, then stir magnetically at a speed of 600r / min for 15min, and centrifuge and dry to obtain stabilized magnesium oxide.

[0092] S4: Assembling stabilized MgO and nano-MgO

[0093] S4.1: Add 10% of the system volume of deionized water to the stabilized magnesium oxide to form a wet sample, press the wet sample into flakes, dry at 60°C, and crush the dried flakes into 1-4 mm particles to obtain stabilized magnesium oxide particles;

[0094] S4.2: Mix nano magnesium oxide and stabilized magnesium oxide particles in a mass ratio of 2:1 to obtain magnesium oxide for low-temperature and high magnetic induction oriented silicon steel.

[0095] Comparative Example 1:

[0096] Comparative Example 1 is commercially available magnesium oxide.

[0097] Comparative Example 2:

[0098] Compared with Example 1, the difference of Comparative Example 2 is that step S3 is not performed to stabilize magnesium oxide, and the nano magnesium oxide of step S2 is directly used, specifically: "S4.1: adding 10% of the system volume of deionized water to the nano magnesium oxide to form a wet sample, and pressing the wet sample into flakes, drying at 50° C., and crushing the dried flakes into 1-4 mm particles to obtain nano magnesium oxide particles;

[0099] S4.2: Mix nano magnesium oxide and nano magnesium oxide particles in a mass ratio of 2:1 to obtain magnesium oxide for low-temperature and high magnetic induction oriented silicon steel. The prepared magnesium oxide for low-temperature and high magnetic induction oriented silicon steel is recorded as Comparative Example 2.

[0100] Comparative Example 3:

[0101] Compared with Example 1, the difference of Comparative Example 3 is that nano magnesium oxide is not prepared, but stabilized magnesium oxide is directly used, specifically: "S4.1: adding 10% of the system volume of deionized water to the stabilized magnesium oxide to form a wet sample, and pressing the wet sample into flakes, drying at 50° C., and crushing the dried flakes into 1-4 mm particles to obtain stabilized magnesium oxide particles;

[0102] S4.2: The stabilized magnesium oxide and the stabilized magnesium oxide particles are mixed in a mass ratio of 2:1 to obtain magnesium oxide for low-temperature and high magnetic induction oriented silicon steel. The prepared new raw material for Poria cultivation is recorded as Comparative Example 3.

[0103] The citric acid activity (CAA 40%) values ​​of Examples 1-3 and Comparative Examples 1-3 were tested, as shown in Table 1.

[0104] Table 1

[0105] CAA40%(s) Example 1 156 Example 2 160 Example 3 181 Comparative Example 1 109 Comparative Example 2 45 Comparative Example 3 313

[0106] The higher the citric acid activity value, the lower the magnesium oxide activity. Excessive magnesium oxide activity is not conducive to the release of gas phase N in low-temperature and high magnetic induction oriented silicon steel. The CAA40% of Example 1 is 156s, the CAA40% of Example 2 is 160s, and the CAA40% of Example 3 is 181s. The CAA40% of high-activity magnesium oxide is 40-300s. It can be seen that the present invention controls the activity of magnesium oxide at a medium level, while the CAA40% of Comparative Example 1 is 109. Compared with the commercially available magnesium oxide in Comparative Example 1, the magnesium oxide of the present invention is less active, but it is still evaluated as highly active magnesium oxide, and will not affect the formation of a magnesium silicate bottom layer of low-temperature and high magnetic induction oriented silicon steel.

[0107] The CAA40% of Comparative Example 2 is 45. It can be seen that nano-magnesium oxide has a very high activity, so it will adsorb gas-phase N, which is not conducive to the release of gas-phase N in low-temperature and high-magnetic induction oriented silicon steel.

[0108] The CAA40% of Comparative Example 3 is 313. It can be seen that the operation of stabilizing magnesium oxide can significantly reduce the activity of magnesium oxide. However, low-activity magnesium oxide is prone to invisible crystal dew or spot-shaped gold dew defects when forming a magnesium silicate bottom layer. The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.

Claims

1. A method for preparing magnesium oxide for low-temperature and high-magnetic-induction oriented silicon steel, characterized in that: The steps include: S1: Preparation of magnesium oxide crystal precursor Weighing MgCl2·6H2O and AlCl3·6H2O and ultrasonically dissolving them in deionized water, and then weighing urea and ultrasonically dissolving them in deionized water to obtain a mixed solution, transferring the mixed solution to a polytetrafluoroethylene reactor for reaction, and then naturally cooling it to room temperature to obtain a suspension, centrifuging the suspension, and then washing the precipitate with deionized water, drying the washed precipitate, and then taking it out and grinding it to obtain a magnesium oxide crystal precursor; S2: Preparation of Nano-MgO The magnesium oxide crystal precursor is evenly spread on the bottom of the magnetic boat, and the magnetic boat is placed in a muffle furnace for calcination to obtain magnesium oxide powder in the magnetic boat. After the magnetic boat is taken out, the magnesium oxide powder is allowed to stand and cool to room temperature, and then ultrasonically dispersed to obtain nano magnesium oxide. S3: Stabilization of magnesium oxide The magnesium oxide powder, sodium nitrate and sodium carbonate are crushed and mixed to obtain a mixed powder, the mixed powder is added to an ethanol dispersant for impregnation, and then vacuum dried to obtain a composite magnesium oxide powder, and then the composite magnesium oxide powder is added to polyvinyl alcohol, the temperature is increased, and ammonia water is added dropwise to adjust the pH, and then magnetic stirring is performed, and centrifugal drying is performed to obtain stabilized magnesium oxide; S4: Assembling stabilized MgO and nano-MgO Deionized water is added to the stabilized magnesium oxide to form a wet sample, and the wet sample is pressed into thin slices, dried, and the dried thin slices are broken to obtain stabilized magnesium oxide particles. Nano-magnesium oxide is mixed with the stabilized magnesium oxide particles to obtain magnesium oxide for low-temperature and high magnetic induction oriented silicon steel.

2. The method for preparing magnesium oxide for low-temperature and high-magnetic induction oriented silicon steel according to claim 1, characterized in that: Step S1 prepares a magnesium oxide crystal precursor, comprising the following steps: S1.1: Weigh 10-12 parts by mass of MgCl2·6H2O and 5-6 parts by mass of AlCl3·6H2O and dissolve them in deionized water by ultrasonic, and then weigh 20-22 parts by mass of urea and dissolve them in deionized water by ultrasonic to obtain a mixed solution; S1.2: The mixed solution is transferred to a polytetrafluoroethylene reactor, reacted at 180-200°C for 30-32 hours, and then naturally cooled to room temperature to obtain a suspension; S1.3: Centrifuge the suspension at 3900-4000 r / min for 3-5 min, and then wash the precipitate with deionized water until the washing solution is neutral; S1.4: The washed precipitate is placed in an oven at 70-80°C and dried for 20-24 hours, then taken out and ground through a 120-mesh sieve to obtain a magnesium oxide crystal precursor.

3. The method for preparing magnesium oxide for low-temperature and high-magnetic-induction oriented silicon steel according to claim 2, characterized in that: In step S1.1, the Mg2+ concentration of MgCl2·6H2O is 0.2 mol / L, and the Al3+ concentration of AlCl3·6H2O is 0.1 mol / L.

4. The method for preparing magnesium oxide for low-temperature and high-magnetic-induction oriented silicon steel according to claim 3, characterized in that: The urea concentration in step S1.1 is 2 mol / L.

5. The method for preparing magnesium oxide for low-temperature and high-magnetic-induction oriented silicon steel according to claim 4, characterized in that: Step S2 is to prepare nano magnesium oxide, comprising the following steps: S2.1: Spread the magnesium oxide crystal precursor evenly on the bottom of the magnetic boat with a thickness of 5-10 mm, place the magnetic boat in a muffle furnace, and calcine at a temperature of 550-580°C for 3-3.2 h with a heating rate of 10°C / min and an initial temperature of 20°C to obtain magnesium oxide powder in the magnetic boat; S2.2: After taking out the magnetic boat, let the magnesium oxide powder stand for 10-20 minutes to cool to room temperature, and then ultrasonically disperse it for 20-30 minutes to obtain nano magnesium oxide.

6. The method for preparing magnesium oxide for low-temperature and high-magnetic-induction oriented silicon steel according to claim 5, characterized in that: Step S3 stabilizes magnesium oxide, comprising the following steps: S3.1: crushing magnesium oxide powder, sodium nitrate and sodium carbonate and mixing them to obtain a mixed powder, adding the mixed powder into an ethanol dispersant, immersing at 75-80° C. for 10-12 hours, and then vacuum drying at 100-120° C. for 24-26 hours to obtain composite magnesium oxide powder; S3.2: Add the composite magnesium oxide powder to 15wt% polyvinyl alcohol, raise the temperature to 50-60°C, add ammonia water to adjust the pH to 10, and then stir magnetically at a speed of 500-600r / min for 15-30min, centrifuge and dry to obtain stabilized magnesium oxide.

7. The method for preparing magnesium oxide for low-temperature and high-magnetic-induction oriented silicon steel according to claim 6, characterized in that: The mass ratio of magnesium oxide, sodium nitrate and sodium carbonate is 30:2:

1.

8. The method for preparing magnesium oxide for low-temperature and high-magnetic-induction oriented silicon steel according to claim 7, characterized in that: The solid-liquid ratio of the mixed powder and the ethanol dispersant is 1:

3.

9. The method for preparing magnesium oxide for low-temperature and high-magnetic-induction oriented silicon steel according to claim 8, characterized in that: The material-liquid ratio of composite magnesium oxide powder and polyvinyl alcohol is 1:

5.

10. The method for preparing magnesium oxide for low-temperature and high-magnetic-induction oriented silicon steel according to claim 9, characterized in that: Step S4 assembling stabilized magnesium oxide and nano magnesium oxide comprises the following steps: S4.1: Add 10% of the system volume of deionized water to the stabilized magnesium oxide to form a wet sample, press the wet sample into flakes, dry at 50-60° C., and crush the dried flakes into 1-4 mm particles to obtain stabilized magnesium oxide particles; S4.2: Mix nano magnesium oxide and stabilized magnesium oxide particles in a mass ratio of 2:1 to obtain magnesium oxide for low-temperature and high magnetic induction oriented silicon steel.

Citation Information

Patent Citations

  • Method for preparing silicon steel magnesium oxide by taking dolomite and bischofite as raw materials

    CN114573009A