Preparation method of scandium-containing aluminate for low-evapotranspiration impregnated diffusion cathode

By doping scandium oxide and europium oxide in 411 aluminate, the scandium-containing aluminate cathode was prepared, which solved the problems of large emission and long life in vacuum electronic devices, improved the emission current density and reduced the evaporation rate, and extended the The service life of the cathode is suitable for industrial promotion.

CN118993132APending Publication Date: 2024-11-22UNIV OF ELECTRONICS SCI & TECH OF CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411100714.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing impregnated diffusion cathodes are difficult to meet the requirements of large emission and long life in high-frequency, high-power vacuum electronic devices, and the evaporation in a vacuum environment affects the device, resulting in device failure.

Method used

Doping scandium oxide and europium oxide in 411 aluminate, scandium-containing aluminate is prepared by ball milling and high-temperature sintering processes to increase the emission current density and reduce the evaporation rate.

Benefits of technology

The high emission current density is improved while reducing the evaporation rate of the cathode, extending the service life of the cathode, and simplifying the preparation process, which is suitable for industrial promotion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993132A_ABST
    Figure CN118993132A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of scandium-containing aluminate for a low-evapotranspiration impregnation diffusion cathode, and belongs to the technical field of manufacturing of vacuum electronic devices. The scandium element and the europium element are doped on the basis of the 411 aluminate, the current emission density of the 411 aluminate is increased by doping the scandium element, and the evaporation rate of the 411 aluminate is reduced by doping the europium element on the basis. Compared with a cathode prepared by using traditional 411 aluminate, the cathode prepared by using the 411 aluminate doped with scandium element and europium element has the advantages that the emission current density is improved, and meanwhile, the maximum evaporation rate is reduced. In addition, the method adopted by the invention has the advantages of simple preparation process, good repeatability and the like, and is suitable for industrial popularization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of vacuum electronic device manufacturing, and relates to a method for preparing an active material for a low evaporation impregnation diffusion cathode, and specifically to a method for preparing aluminate formed by doping a certain proportion of europium oxide and scandium oxide on a 411 aluminate component. Background Art

[0002] With the rapid development of science and technology, especially in cutting-edge fields such as aerospace, communications and medical treatment, the demand for high-performance and high-reliability vacuum electronic devices is becoming increasingly urgent. As the core component of these devices, the cathode plays a vital role. In order to promote vacuum electronic devices to higher frequencies and higher powers, it is imperative to develop cathode electron sources with high emission current density and long life.

[0003] At present, the impregnated diffusion cathode has been widely used in modern vacuum electronic devices. It is mainly composed of a refractory metal substrate and an active emission material impregnated therein; the porous metal substrate acts as a reservoir, and the active emission material diffuses from the pores to the surface to maintain the active layer, thereby providing a low work function surface for thermal electron emission and making it possible for large current emission. However, its current performance is still difficult to meet the stringent requirements of devices for large emission and long life. The end of the cathode life is mainly affected by the evaporation of the emission material. In addition to affecting the life of the cathode, the cathode operating in a vacuum environment will release evaporants that will have varying degrees of impact on adjacent components. These impacts may manifest as sparking, poisoning, and other failure modes of the device, ultimately affecting the use of the vacuum device.

[0004] In order to increase the emission of the cathode and reduce evaporation, researchers have selected a highly emitting impregnated active salt: 411 aluminate (the numbers represent the molar ratio of BaCO3, CaCO3, and Al2O3). The study found that the addition of scandium can effectively increase the current emission density of the cathode; however, the stability of the scandium-containing aluminate cathode is poor, which affects the actual use of vacuum devices. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention provides a method for preparing a scandium-containing aluminate doped with europium to achieve low evaporation for an impregnated diffusion cathode. The present invention adds an appropriate amount of scandium oxide and europium oxide to 411 aluminate, so that the scandium-containing aluminate can maintain a high emission current density while reducing the evaporation of the impregnated active material, thereby extending the service life of the cathode.

[0006] The technical solution adopted by the present invention is as follows:

[0007] A method for preparing a scandium-containing aluminate for a low evaporation impregnation diffusion cathode comprises the following steps:

[0008] S1. Place sufficient amounts of analytically pure BaCO3, CaCO3, Al2O3, Sc2O3 and Eu2O3 in a forced air drying oven and dry them.

[0009] S2. Calculate and weigh BaCO3, CaCO3, and Al2O3 in step S1 according to the molar ratio of BaO:CaO:Al2O3 = 4:1:1; then weigh Sc2O3 and Eu2O3 in proportion, wherein the mass of Sc2O3 accounts for 1wt.% to 3wt.% of the total mass, and the mass of Eu2O3 accounts for 1wt.% to 3wt.% of the total mass.

[0010] S3. The weighed raw materials are mixed by ball milling using a planetary ball mill to obtain a mixed powder.

[0011] S4. The mixed powder is sieved by sampling to obtain a precursor powder; the precursor powder is placed in a mold, and pressed into a round cake-shaped mixture by a tablet press.

[0012] S5. The round cake-shaped mixture is subjected to high-temperature sintering. According to the decomposition behavior of barium carbonate, the sintering conditions are set as follows: keeping the temperature at 850°C to 855°C for 2 to 3 hours; then heating the temperature to 1200°C to 1300°C at a heating rate of 2°C / min, keeping the temperature for 300 minutes to 360 minutes; and finally cooling the mixture naturally.

[0013] S6. Grind the sintered round cake-shaped mixture into powder to obtain scandium-containing aluminate for impregnation diffusion cathode.

[0014] Preferably, in step S1, the drying condition is: drying at 100°C to 120°C for more than 24 hours.

[0015] Preferably, in step S3, the ball milling time is more than 24 hours.

[0016] Preferably, in step S4, when the precursor powder is pressed by a tablet press, the pressure is set to 20 MPa to 30 MPa.

[0017] Preferably, in step S5, the disc is subjected to high-temperature sintering by placing the disc-shaped mixture in a crucible and then placing it in a muffle furnace for high-temperature sintering.

[0018] Beneficial effects of the present invention:

[0019] The present invention doped scandium and europium on the basis of 411 aluminate, increased its current emission density by doping scandium, and on this basis doped europium to reduce the evaporation rate of 411 aluminate. The results show that compared with the cathode prepared by using traditional 411 aluminate, the cathode prepared by using 411 aluminate doped with scandium and europium in the present invention increases the emission current density and reduces the maximum evaporation rate. In addition, the method used in this invention has the advantages of simple preparation process, good repeatability, etc., and is suitable for industrial promotion. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Attached Figure 1 Powder X-ray diffraction spectra of scandium aluminate when the Sc2O3 content is 1wt.%, 2wt.%, and 3wt.%, respectively.

[0021] Figure 2 (a) shows the DC emission current density J (in A / cm2) of the impregnated 411 aluminate cathode. 2 ) and the logarithm of voltage U (unit V).

[0022] Figure 2 (b) shows the DC emission current density J (in A / cm2) of the cathode impregnated with 411 aluminate and 3 wt.% Sc2O3 2 ) and the logarithm of voltage U (unit V).

[0023] Figure 2 (c) shows the DC emission current density J (in A / cm2) of the cathode impregnated with 411 aluminate and added with 2wt.% Sc2O3 and 1wt.% Eu2O3. 2 ) and the logarithm of voltage U (unit V).

[0024] Figure 2 (d) DC emission current density J (unit A / cm2) of the cathode impregnated with 411 aluminate with 1wt.% Sc2O3 and 2wt.% Eu2O3 2 ) and the logarithm of voltage U (unit V). DETAILED DESCRIPTION

[0025] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings.

[0026] This embodiment provides a method for preparing a scandium-containing aluminate for a low evaporation impregnation diffusion cathode, comprising the following steps:

[0027] S1. Place sufficient amounts of analytically pure BaCO3, CaCO3, Al2O3, Sc2O3 and Eu2O3 in a forced air drying oven and dry at 120°C for 24 hours.

[0028] S2. Calculate and weigh BaCO3, CaCO3, and Al2O3 in step S1 according to the molar ratio of BaO:CaO:Al2O3=4:1:1; then weigh Sc2O3 and Eu2O3 according to the mass ratio, wherein the mass of Sc2O3 is x wt.%, and the mass of Eu2O3 is (3-x) wt.%, and x=1, 2, 3, thus obtaining 3 groups of raw materials with different ratios.

[0029] S3. Three groups of raw materials with different proportions were mixed by ball milling using a planetary ball mill for 24 hours to obtain three groups of mixed powders.

[0030] S4. Separate the three groups of mixed powders using a sample sieve to obtain three groups of precursor powders; put the three groups of precursor powders into a mold respectively, set the tablet press pressure to 30 MPa, and press to obtain four round cake-shaped mixtures with a diameter of 10 mm.

[0031] S5. The three round cake-shaped mixtures were sintered at high temperature. According to the decomposition behavior of barium carbonate, the sintering conditions were set as follows: keeping the temperature at 850°C for 3 hours; then heating to 1200°C at a heating rate of 2°C / min and keeping the temperature for 300 minutes; and finally cooling naturally.

[0032] S6. The three sintered round cake-shaped mixtures were ground into powder using an agate mortar to obtain three aluminates with different ratios for impregnation diffusion cathode.

[0033] X-ray diffraction analysis was performed on the three prepared doped aluminates with different ratios:

[0034] The conditions for diffraction data collection are: sampling time 1 second, sampling step width 0.02°, and Bragg diffraction angle range 5°~90°. Figure 1 This is the comparison of X-ray diffraction data of four samples. After comparison by phase analysis software, it can be seen that the four aluminates all contain Ba3CaAl2O7 and Ba4Al2O7. The most important thing is that Ba3CaAl2O7 is an effective electron emission active substance. After entering the cathode tungsten sponge matrix, it can react efficiently with the tungsten matrix to increase the emission current density of the cathode.

[0035] The cathode was impregnated with 3 different ratios of doped aluminates:

[0036] A cylindrical tungsten sponge with a porosity of 25-30%, a diameter of 3mm and a thickness of 2mm is selected as the cathode substrate, and a molybdenum support tube, molybdenum-ruthenium solder, alumina powder and a heating wire are prepared. The cathode substrate and the molybdenum support tube are brazed at a high temperature of 1980°C with molybdenum-ruthenium solder to ensure that the two are tightly combined; then the heating wire is placed in the molybdenum support tube, and alumina powder is filled around the heating wire to provide necessary support and insulation, and high-temperature sintering is performed at 1700°C for 2-3 minutes to densify the alumina powder and fix the position of the heater.

[0037] The cathode substrate was placed upside down in the emission material, and a high-temperature hydrogen furnace was used to raise the temperature to 1690°C in a H2 atmosphere, and the temperature was kept for about 5 minutes for impregnation. After the impregnation, the cathode assembly was taken out, the residual salt and impurities on the surface were removed, and the surface was polished to obtain a smooth and uniform cathode surface, and finally a test cathode was made. The emission materials were 411 aluminate powder and three different ratios of doped aluminate powders (411 aluminate with x wt.% Sc2O3 and (3-x) wt.% Eu2O3 (x=1,2,3) added according to the mass ratio), that is, four different impregnated cathodes were prepared.

[0038] Impregnation cathode pretreatment:

[0039] Prepare the water-cooled copper anode diode assembly and ensure it is in good working condition. Install the prepared cathode assembly into the test device, ensuring that the distance and position from the anode meet the test requirements. -6 Pa), turn on the test device and heat the cathode to 1150°C B (Brightness temperature), activate the cathode for more than 2 hours, and then record the data after the emission current stabilizes.

[0040] Electron emission test:

[0041] After the cathode is activated, the temperature of the immersed cathode is adjusted to the preset temperature (such as 1100℃, 1050℃, 1000℃), and then the anode voltage is adjusted at equal intervals of 20V, and the data is recorded after the current emission is stable. Due to the electron cooling effect in DC mode, the temperature of the cathode surface will decrease, so temperature compensation is used for electron emission measurement.

[0042] Figure 2 (a) shows the DC emission current density J (in A / cm2) of the impregnated 411 aluminate cathode. 2 ) and voltage U (unit V) logarithm, and the DC emission current density is determined to be 6.347 A / cm at 1100°C according to the method of deviation from the space charge confinement region. 2 .

[0043] Figure 2(b) shows the DC emission current density J (in A / cm2) of the cathode impregnated with 411+3wt.%Sc2O3 aluminate. 2 ) vs. voltage U (unit V), we can see that after adding 3wt.% Sc2O3 to 411 aluminate, the DC current emission density increased to 9.148A / cm at 1100℃ 2 , the emission capacity of the cathode has been significantly enhanced.

[0044] Figure 2(c) is a graph showing the logarithm of the DC emission current density J (in A / cm2) and the logarithm of the voltage U (in V) of the aluminate cathode impregnated with 411+2wt.%Sc2O3+1wt.%Eu2O3. It can be seen that after adding 2wt.%Sc2O3 and 1wt.%Eu2O3 to 411 aluminate, the DC current emission density is 8.681A / cm2 at 1100°C. 2 , compared with 411 aluminate, the emission capability is significantly improved.

[0045] Figure 2(d) is a graph showing the logarithm of the DC emission current density J (in A / cm2) and the logarithm of the voltage U (in V) of the aluminate cathode impregnated with 411+1wt.%Sc2O3+2wt.%Eu2O3. It can be seen that after adding 1wt.%Sc2O3 and 2wt.%Eu2O3 to the 411 aluminate cathode, the DC current emission density is 7.211A / cm2 at 1100°C. 2 , the launch capability is still significantly improved compared with 411 aluminate.

[0046] Table 1 Comparison of cathode emission density

[0047]

[0048] Evaporation rate test:

[0049] A molybdenum sheet was placed 8.5 mm in front of the cathode emission to allow the evaporated material to evaporate onto the molybdenum sheet. Finally, the evaporation rates of the doped aluminate impregnated cathodes with different ratios were obtained as shown in Table 2.

[0050] Table 2 Comparison of cathode evaporation rates

[0051] Cathode Type Evaporation rate (nm / h) Evapotranspiration thickness (nm) <![CDATA[Impregnated 411 + 3 wt.% Sc2O3 cathode]]> 1.38~1.57 156~177 <![CDATA[Impregnated 411 + 2 wt.% Sc2O3 + 1 wt.% Eu2O3 cathode]]> 1.14~1.31 134~154 <![CDATA[Impregnated 411 + 1 wt.% Sc2O3 + 2 wt.% Eu2O3 cathode]]> 1.0~1.24 128~150

[0052] From Table 1 and Table 2, it can be seen that the emission capacity of the cathode impregnated with 411 aluminate is significantly enhanced after adding Sc2O3, especially the emission capacity of the cathode impregnated with 411 aluminate with 3wt.% Sc2O3 is increased from 6.347A / cm2 to 411 aluminate. 2 Improved to 9.148A / cm 2; With the increase of europium content, it can be seen that its evaporation rate is gradually decreasing. When 1wt.% Eu2O3 and 2wt.% Sc2O3 are added, the emission performance and low evaporation characteristics are significantly improved compared with 411 aluminate. It can be seen that according to the needs of cathode current emission density and evaporation rate, the appropriate addition ratio of Sc2O3 and Eu2O3 can be selected, so that the cathode has a better emission and the evaporation rate is significantly reduced.

Claims

1. A method for preparing a scandium-containing aluminate for a low evaporation impregnation diffusion cathode, characterized in that: The following steps are involved: S1. Place sufficient amounts of analytically pure BaCO3, CaCO3, Al2O3, Sc2O3 and Eu2O3 in a blast drying oven to dry; S2. Calculate and weigh BaCO3, CaCO3, Al2O3 in step S1 according to the molar ratio of BaO:CaO:Al2O3 = 4:1:1; then weigh Sc2O3 and Eu2O3 in proportion, wherein the mass of Sc2O3 accounts for 1wt.% to 3wt.% of the total mass, and the mass of Eu2O3 accounts for 1wt.% to 3wt.% of the total mass; S3. The weighed raw materials were mixed by ball milling in a planetary ball mill to obtain a mixed powder; S4. The mixed powder is sieved by a sample to obtain a precursor powder; the precursor powder is placed in a mold and pressed into a round cake-shaped mixture by a tablet press; S5. The round cake-shaped mixture is sintered at high temperature, and the sintering conditions are set as follows: at about 850 ℃ ~ 855 ℃, keep warm for 2 to 3 hours; then heat up to 1200 ℃ ~ 1300 ℃ at a heating rate of 2 ℃ / min, keep warm for 300 minutes ~ 360 minutes; finally cool naturally; S6. Grind the sintered round cake-shaped mixture into powder to obtain scandium-containing aluminate for impregnation diffusion cathode.

2. The method for preparing a scandium-containing aluminate for a low evaporation impregnation diffusion cathode according to claim 1, characterized in that: In step S1, the drying condition is: drying at 100°C to 120°C for more than 24 hours.

3. The method for preparing a scandium-containing aluminate for a low evaporation impregnation diffusion cathode according to claim 1, characterized in that: In step S3, the ball milling time is more than 24 hours.

4. The method for preparing a scandium-containing aluminate for a low evaporation impregnation diffusion cathode according to claim 1, characterized in that: In step S4, when the precursor powder is pressed by a tablet press, the pressure is set to 20 MPa to 30 MPa.

5. The method for preparing a scandium-containing aluminate for a low evaporation impregnation diffusion cathode according to claim 1, characterized in that: In step S5, the disc is subjected to high-temperature sintering in the following manner: the disc-shaped mixture is placed in a crucible, and then placed in a muffle furnace for high-temperature sintering.