Treatment method for recycling anhydrous cupric sulfate from mixed acidic and alkaline copper-containing waste etching liquid
Through the self-heating mixed acidic and alkaline copper-containing waste etching liquid recovery method, the neutralization tank and pH value detection are used to solve the problems of high treatment cost of acidic and alkaline waste liquid and large equipment occupation, and high quality and no-quality The recycling of water copper sulfate optimizes production costs and site utilization.
Patent Information
- Application Number
- CN202411112480.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-22
AI Technical Summary
In the prior art, the treatment of acidic and alkaline copper-containing waste etching liquid requires the configuration of treatment agents and special equipment respectively, resulting in high costs and large equipment occupation, which affects the production cost of the enterprise and the site utilization efficiency.
The self-heating mixed acidic and alkaline copper-containing waste etching liquid recovery method is adopted. By setting up a neutralization tank and a neutralization platform, the heat generated by the neutralization reaction is used for self-heating, and combined with pH detection and the regulation of the conveying pump. Achieve the recycling of anhydrous copper sulfate and reduce equipment investment and site occupation.
It effectively reduces the treatment cost of acidic and alkaline copper-containing waste etching liquid, reduces the demand for special equipment, optimizes production costs and site utilization, and achieves high-quality recycling of anhydrous copper sulfate.
Smart Images

Figure HDA0004992648480000011
Abstract
Description
Technical Field
[0001] The invention relates to waste recycling technology and recycling equipment, and specifically to a treatment method for recycling anhydrous copper sulfate from mixed acidic and alkaline copper-containing waste etching liquid. Background Art
[0002] The treatment of copper-containing etching waste liquid has always been a major problem faced by printed circuit board companies. The copper-containing etching waste liquid is determined by the printing process, including acidic copper-containing waste etching liquid after acid etching and alkaline copper-containing waste etching liquid after alkaline etching. At this stage, the acidic copper-containing waste etching liquid after acid etching and the alkaline copper-containing waste etching liquid after alkaline etching are generally treated separately. The treatment requires the configuration of treatment agents and special equipment respectively, resulting in high treatment costs for the acidic copper-containing waste etching liquid after acid etching and the alkaline copper-containing waste etching liquid after alkaline etching, and multiple equipment occupies a large site, which is not conducive to the optimization of production costs and the implementation of production sites by enterprises.
[0003] Therefore, it is necessary to provide a treatment method for recovering anhydrous copper sulfate from mixed acidic and alkaline copper-containing waste etching liquid to achieve the above purpose. Summary of the invention
[0004] The invention aims to provide a treatment method for recovering anhydrous copper sulfate from mixed acidic and alkaline copper-containing waste etching liquid.
[0005] The present invention achieves the above object through the following technical solutions:
[0006] A method for recovering anhydrous copper sulfate from mixed acidic and alkaline copper-containing waste etching liquid, comprising:
[0007] 1) a neutralization tank is provided, wherein a neutralization platform is provided in the neutralization tank; the neutralization platform comprises a lower bearing platform for receiving one of the acidic copper-containing waste etching solution or the alkaline copper-containing waste etching solution, and an upper bearing platform for receiving the other of the acidic copper-containing waste etching solution or the alkaline copper-containing waste etching solution is provided corresponding to the lower bearing platform;
[0008] 2) A waste liquid retention tank is provided in the middle of the lower bearing platform, and one of the acidic copper-containing waste etching liquid or the alkaline copper-containing waste etching liquid is fed into the waste liquid retention tank at a rate of no more than 2 liters / min, and the current pH value of the influent liquid is recorded, which is recorded as A;
[0009] 3) Adding acidic copper-containing waste etching solution or alkaline copper-containing waste etching solution to another corresponding upper carrier, testing the pH value of the current upper liquid body, recorded as B, comparing the ratio of A to B, and obtaining the liquid speed of the upper carrier;
[0010] 4) Corresponding to the waste liquid retention tank, a waste liquid neutralization slope is arranged on the upper bearing platform to form a retention type pre-neutralized acidic copper-containing waste etching liquid or alkaline copper-containing waste etching liquid recovery structure;
[0011] 5) The incompletely neutralized acidic copper-containing waste etching solution or alkaline copper-containing waste etching solution continues to flow into the neutralization tank for neutralization;
[0012] 6) Acidic copper-containing waste etching liquid or alkaline copper-containing waste etching liquid generates a large amount of heat. The neutralization tank is set in a closed form, and the heat generated by neutralization is used as feedback to heat the neutralized aqueous copper sulfate, forming a self-heating mixed acidic and alkaline copper-containing waste etching liquid to recover anhydrous copper sulfate. A heating element is also set in the neutralization tank for auxiliary heating to form a high-quality anhydrous copper sulfate recovery method.
[0013] Furthermore, the lower supporting platform is also provided with a downward slope for neutralizing the waste liquid.
[0014] Furthermore, the acidic copper-containing waste etching liquid is input into the lower supporting platform or the upper supporting platform through the waste acid delivery pipe.
[0015] Furthermore, a waste acid pH value detector is provided on the waste acid delivery pipe, and an acidic copper-containing waste etching liquid delivery pump is also provided to cooperate with the waste acid pH value detector.
[0016] Furthermore, the alkaline copper-containing waste etching solution is input into the lower supporting platform or the upper supporting platform through the waste alkali conveying pipe.
[0017] Furthermore, a waste alkali pH value detector is provided on the waste alkali conveying pipe, and an alkaline copper-containing waste etching liquid conveying pump matched with the waste alkali pH value detector is also provided.
[0018] Furthermore, the acidic copper-containing waste etching liquid delivery pump and the alkaline copper-containing waste etching liquid delivery pump are used to adjust the delivery speed based on the detection data of the waste acid pH value detector and the waste alkali pH value detector, so as to form an adaptive and adjustable structure of the acidic copper-containing waste etching liquid and the alkaline copper-containing waste etching liquid.
[0019] Furthermore, a high-power exhaust fan module is provided on the top of the neutralization tank.
[0020] Compared with the prior art, the present invention realizes the recovery of anhydrous copper sulfate by mixing acidic and alkaline copper-containing waste etching liquids through a self-heating mixed acidic and alkaline copper-containing waste etching liquid, effectively reduces the treatment cost of acidic copper-containing waste etching liquid or alkaline copper-containing waste etching liquid, and reduces the investment in special equipment and site occupation, which is convenient for enterprises to optimize the implementation of production costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a structural schematic diagram of the present invention. DETAILED DESCRIPTION
[0022] Example:
[0023] See also Figure 1 This embodiment is a method for recovering anhydrous copper sulfate from a mixed acidic and alkaline copper-containing waste etching solution, the steps comprising:
[0024] 1) a neutralization tank 1 is provided, wherein a neutralization platform is provided in the neutralization tank 1; the neutralization platform comprises a lower support platform 2 for receiving one of the acidic copper-containing waste etching solution or the alkaline copper-containing waste etching solution, and an upper support platform 3 for receiving the other of the acidic copper-containing waste etching solution or the alkaline copper-containing waste etching solution is provided corresponding to the lower support platform 2;
[0025] 2) A waste liquid retention tank 21 is provided in the middle of the lower supporting platform 2, and one of the acidic copper-containing waste etching liquid or the alkaline copper-containing waste etching liquid is fed into the waste liquid retention tank at a feeding speed of no more than 2 liters / min, and the current pH value of the influent is recorded, which is recorded as A;
[0026] 3) Adding acidic copper-containing waste etching solution or alkaline copper-containing waste etching solution to another corresponding upper carrier 3, testing the pH value of the current upper liquid body, recorded as B, comparing the ratio of A to B, and obtaining the liquid speed of the upper carrier 3;
[0027] 4) Corresponding to the waste liquid retention tank 21, a waste liquid neutralization slope 31 is provided on the upper supporting platform 3 to form a retention type pre-neutralized acidic copper-containing waste etching liquid or alkaline copper-containing waste etching liquid recovery structure;
[0028] 5) The incompletely neutralized acidic copper-containing waste etching solution or alkaline copper-containing waste etching solution continues to flow into the neutralization tank 1 for neutralization;
[0029] 6) Acidic copper-containing waste etching liquid or alkaline copper-containing waste etching liquid generates a large amount of heat. The neutralization tank 1 is set in a closed form, and the heat generated by neutralization is used as feedback to heat the neutralized aqueous copper sulfate, forming a self-heating mixed acidic and alkaline copper-containing waste etching liquid to recover anhydrous copper sulfate. A heating element is also set in the neutralization tank 1 for auxiliary heating to form a high-quality anhydrous copper sulfate recovery method.
[0030] The lower supporting platform 2 is also provided with a downstream slope 22 for neutralizing waste liquid.
[0031] The acidic copper-containing waste etching liquid is input into the lower supporting platform 2 or the upper supporting platform 3 through the waste acid delivery pipe 4 .
[0032] The waste acid delivery pipe 4 is provided with a waste acid pH value detector 41 , and is also provided with an acidic copper-containing waste etching liquid delivery pump matched with the waste acid pH value detector 41 .
[0033] The alkaline copper-containing waste etching solution is input into the lower supporting platform 2 or the upper supporting platform 3 through the waste alkali conveying pipe 5 .
[0034] The waste alkali conveying pipe 5 is provided with a waste alkali pH value detector 51 , and is also provided with an alkaline copper-containing waste etching liquid conveying pump matched with the waste alkali pH value detector 51 .
[0035] According to the detection data of the waste acid pH value detector 41 and the waste alkali pH value detector 51, the acidic copper-containing waste etching liquid delivery pump and the alkaline copper-containing waste etching liquid delivery pump adjust the delivery speed to form an adaptively regulated structure of the acidic copper-containing waste etching liquid and the alkaline copper-containing waste etching liquid.
[0036] Corresponding to the neutralization tank 1, a high-power exhaust fan module 6 is provided.
[0037] Compared with the prior art, the present invention realizes mixed neutralization treatment of acidic waste copper-containing etching liquid and alkaline waste copper-containing etching liquid without other metal substances through the retention type pre-neutralization harmless disposal structure of mixed acidic waste copper-containing etching liquid and alkaline waste copper-containing etching liquid, and effectively reduces the treatment cost of acidic waste copper-containing etching liquid and alkaline waste copper-containing etching liquid.
[0038] The above are only some embodiments of the present invention. For those skilled in the art, several modifications and improvements can be made without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A method for recovering anhydrous copper sulfate from a mixed acidic and alkaline copper-containing waste etching solution, characterized in that: include: 1) a neutralization tank is provided, wherein a neutralization platform is provided in the neutralization tank; the neutralization platform comprises a lower bearing platform for receiving one of the acidic copper-containing waste etching solution or the alkaline copper-containing waste etching solution, and an upper bearing platform for receiving the other of the acidic copper-containing waste etching solution or the alkaline copper-containing waste etching solution is provided corresponding to the lower bearing platform; 2) A waste liquid retention tank is provided in the middle of the lower bearing platform, and one of the acidic copper-containing waste etching liquid or the alkaline copper-containing waste etching liquid is fed into the waste liquid retention tank at a rate of no more than 2 liters / min, and the current pH value of the influent liquid is recorded, which is recorded as A; 3) Adding acidic copper-containing waste etching solution or alkaline copper-containing waste etching solution to another corresponding upper carrier, testing the pH value of the current upper liquid body, recorded as B, comparing the ratio of A to B, and obtaining the liquid speed of the upper carrier; 4) Corresponding to the waste liquid retention tank, a waste liquid neutralization slope is arranged on the upper bearing platform to form a retention type pre-neutralized acidic copper-containing waste etching liquid or alkaline copper-containing waste etching liquid recovery structure; 5) The incompletely neutralized acidic copper-containing waste etching solution or alkaline copper-containing waste etching solution continues to flow into the neutralization tank for neutralization; 6) Acidic copper-containing waste etching liquid or alkaline copper-containing waste etching liquid generates a large amount of heat. The neutralization tank is set in a closed form, and the heat generated by neutralization is used as feedback to heat the neutralized aqueous copper sulfate, thereby forming a self-heating mixed acidic and alkaline copper-containing waste etching liquid to recover anhydrous copper sulfate.
2. According to the method for recovering anhydrous copper sulfate from a mixed acidic and alkaline copper-containing waste etching solution as described in claim 1, a heating element is also provided in the neutralization tank for auxiliary heating to form a high-quality anhydrous copper sulfate recovery method.
3. A method for recovering anhydrous copper sulfate from a mixed acidic and alkaline copper-containing waste etching solution according to claim 1 or 2, characterized in that: The lower bearing platform is also provided with a downward slope for neutralizing waste liquid.
4. The method for recovering anhydrous copper sulfate from a mixed acidic and alkaline copper-containing waste etching solution according to claim 3, characterized in that: The acidic copper-containing waste etching liquid is input into the lower supporting platform or the upper supporting platform through the waste acid conveying pipe.
5. The method for recovering anhydrous copper sulfate from a mixed acidic and alkaline copper-containing waste etching solution according to claim 4, characterized in that: The waste acid delivery pipe is provided with a waste acid pH value detector, and is also provided with an acidic copper-containing waste etching liquid delivery pump matched with the waste acid pH value detector.
6. The method for recovering anhydrous copper sulfate from a mixed acidic and alkaline copper-containing waste etching solution according to claim 5, characterized in that: The alkaline copper-containing waste etching solution is input into the lower supporting platform or the upper supporting platform through the waste alkali conveying pipe.
7. The method for recovering anhydrous copper sulfate from a mixed acidic and alkaline copper-containing waste etching solution according to claim 6, characterized in that: The waste alkali conveying pipe is provided with a waste alkali pH value detector, and is also provided with an alkaline copper-containing waste etching liquid conveying pump matched with the waste alkali pH value detector.
8. The method for recovering anhydrous copper sulfate from a mixed acidic and alkaline copper-containing waste etching solution according to claim 7, characterized in that: According to the detection data of the waste acid pH value detector and the waste alkali pH value detector, the acidic copper-containing waste etching liquid delivery pump and the alkaline copper-containing waste etching liquid delivery pump adjust the delivery speed to form an adaptive and adjustable structure of the acidic copper-containing waste etching liquid and the alkaline copper-containing waste etching liquid.
9. The method for recovering anhydrous copper sulfate from a mixed acidic and alkaline copper-containing waste etching solution according to claim 8, characterized in that: A high-power exhaust fan module is arranged on the top of the neutralization tank.