Hollow zinc sulfide nanotube for positive electrode of aqueous zinc-sulfur battery and preparation method of hollow zinc sulfide nanotube
By preparing hollow zinc sulfide nanotubes as the positive electrode material of aqueous zinc-sulfur battery, the problem of insufficient volume expansion and kinetics of the positive electrode material is solved, the charging and discharging performance and cycle stability of the battery are improved, and the battery life is extended.
Patent Information
- Application Number
- CN202411229976.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-03
AI Technical Summary
The positive electrode material of aqueous zinc-sulfur battery has problems of volume expansion and insufficient kinetics, resulting in fast battery capacity decay, low Coulomb efficiency and short cycle life.
Hollow zinc sulfide nanotubes are used as the positive electrode material, and through the preparation, surface vulcanization and chemical etching steps of zinc oxide nanorods, a hollow structure with good conductivity is formed, which alleviates volume changes in sulfur oxidation and improves the cycle stability of the battery.
It significantly improves the charge and discharge performance and cycle stability of aqueous zinc-sulfur batteries, extends the battery life, and improves the mechanical stability of the electrode structure.
Smart Images

Figure CN118993137A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aqueous zinc ion batteries, and in particular to a hollow zinc sulfide nanotube for an aqueous zinc-sulfur battery positive electrode and a preparation method thereof. Background Art
[0002] With the rapid development of today's society, economy and technology, all kinds of electronic devices are upgrading towards higher performance, lighter and more portable, which poses a great challenge to the capacity and performance of batteries. Lithium-ion batteries and sodium-ion batteries are the most widely used batteries. However, due to their disadvantages of insecurity, high cost and poor rate performance, the research focus is gradually shifting from lithium-ion batteries and sodium-ion batteries to another emerging battery - aqueous zinc-sulfur batteries.
[0003] Aqueous zinc-sulfur batteries use sulfur as the positive electrode active material and zinc metal sheets as the negative electrode, and complete charging and discharging through the redox process of the positive and negative electrode materials. Aqueous zinc-sulfur batteries have the following advantages over other batteries: 1) Intrinsic safety: Aqueous electrolytes have the characteristics of low toxicity, low volatility, and non-flammable, which improves battery safety. 2) Low cost and environmental friendliness: First, aqueous electrolytes have certain cost advantages over organic electrolytes in terms of solvents and inorganic zinc salts. Secondly, zinc metal and sulfur elements are abundant in the earth's crust. In addition, aqueous zinc-sulfur batteries have relatively little impact on the environment during production and recycling, which reduces production costs. 3) Good rate performance: The ionic conductivity of aqueous electrolytes is high, which can achieve rapid charging and discharging of batteries. 4) High specific capacity: The theoretical specific capacity of sulfur is high, at 1675mAh / g, and the zinc negative electrode also has a theoretical specific capacity of up to 820mAh / g.
[0004] The advantages of zinc-sulfur batteries are very obvious, but there are also problems that need to be solved urgently. The main contradictions are concentrated in the positive electrode materials of zinc-sulfur batteries: 1) Volume expansion: During the dynamic cycle of zinc-sulfur batteries, the sulfur positive electrode will undergo a certain volume change, causing certain mechanical damage and easily leading to the collapse of the electrode structure. 2) Insufficient kinetics: The reactant S8 and the discharge end product ZnS both have low electronic and ionic conductivity, resulting in rapid capacity decay, low coulombic efficiency and short cycle life of the battery.
[0005] Therefore, the industry urgently needs a new technology for positive electrode materials for aqueous zinc-sulfur batteries. Summary of the invention
[0006] In view of the shortcomings of the prior art, the present invention provides a hollow zinc sulfide nanotube for the positive electrode of an aqueous zinc-sulfur battery and a preparation method thereof. The ingenious design of the positive electrode can solve the pain points of the positive electrode materials of aqueous zinc-sulfur batteries. The hollow zinc sulfide nanotube positive electrode not only has good conductivity, can improve polarization, and improve charge and discharge performance; but also can provide space for the volume change of sulfur produced during oxidation, thereby reducing structural damage to the electrode and improving cycle stability.
[0007] The present invention adopts the following technical solution:
[0008] A method for preparing a hollow zinc sulfide nanotube for an aqueous zinc-sulfur battery positive electrode comprises the following steps:
[0009] S1. Preparation of zinc oxide nanorods: 2+ The metal salt is dissolved in an aqueous solution of an alkali metal hydroxide, and after being stirred evenly, a polyol organic solvent is added in proportion, and the mixture is placed in a reactor for hydrothermal reaction to obtain zinc oxide nanorods;
[0010] S2, surface vulcanization: dissolving the zinc oxide nanorods and the vulcanizing agent in the step S1 in a mixed solution of ethanol and water, and then stirring at a certain temperature to perform a vulcanization reaction to obtain a zinc sulfide-coated zinc oxide material;
[0011] S3, chemical etching: the zinc sulfide-coated zinc oxide material in step S2 is uniformly dispersed in an etchant aqueous solution, and then stirred at a certain temperature to perform a chemical etching reaction to obtain a hollow zinc sulfide nanotube material.
[0012] The step S1 contains Zn 2+ The metal salt is at least one of zinc acetate dihydrate, zinc nitrate hexahydrate, zinc chloride, zinc nitrate and zinc sulfate; the Zn-containing 2+ The molar concentration of the metal salt is 0.1 to 0.5 mol / L.
[0013] In step S1, the alkali metal hydroxide is at least one of lithium hydroxide, sodium hydroxide and potassium hydroxide; and the molar concentration of the alkali metal hydroxide is 6 to 10 mol / L.
[0014] In the step S1, the polyol solvent is at least one of ethylene glycol, propylene glycol, and glycerol; the volume ratio between the polyol solvent and the aqueous solution is (2-5):1.
[0015] The temperature of the hydrothermal reaction in step S1 is 120-180° C., and the reaction time is 12-24 hours.
[0016] In step S2, the vulcanizing agent is at least one of thioacetamide, thiourea and sodium sulfide; and the molar ratio between the added zinc oxide nanorods and the vulcanizing agent is (1-12):1.
[0017] The volume ratio of the mixed solution of ethanol and water in step S2 is 1:(2-4).
[0018] The temperature of the sulfurization reaction in step S2 is 60-80° C., and the reaction time is 2-8 hours.
[0019] In step S3, the chemical etchant is at least one of ammonia water, ammonium chloride, sodium hydroxide and potassium hydroxide; the molar concentration of the etchant aqueous solution is 1-3 mol / L.
[0020] The temperature of the chemical etching reaction in step S3 is 60-80° C., and the reaction time is 6-12 hours.
[0021] A hollow zinc sulfide nanotube for the positive electrode of an aqueous zinc-sulfur battery is prepared according to the preparation method.
[0022] The invention discloses an application of the hollow zinc sulfide nanotubes prepared according to the preparation method in an aqueous zinc-sulfur battery. The aqueous zinc-sulfur battery is assembled by using the hollow zinc sulfide nanotubes as a positive electrode, a zinc metal sheet as a negative electrode, a separator and an aqueous electrolyte.
[0023] The hollow zinc sulfide nanotubes are mixed with conductive carbon black and a binder in a certain proportion to prepare a slurry, which is then coated on the surface of a current collector and dried to obtain a positive electrode sheet for an aqueous zinc-sulfur battery.
[0024] The mass ratio of the hollow zinc sulfide nanotube to the conductive carbon black and the binder is one of 9:0.5:0.5, 8:1:1, 7:2:1 and 6:3:1.
[0025] The conductive carbon black is at least one of Super P, acetylene black and Ketjen black.
[0026] The binder is at least one of LA133, sodium alginate, PVDF and PTFE.
[0027] The current collector is at least one of stainless steel foil, stainless steel mesh, titanium foil, titanium mesh, carbon fiber cloth, carbon paper, and graphite paper.
[0028] The diaphragm is at least one of glass fiber, non-woven fabric, and proton exchange membrane;
[0029] The aqueous electrolyte is prepared by dissolving zinc metal salt in deionized water solution, and its concentration is 1-10 mol / L.
[0030] The zinc metal salt is at least one of zinc sulfate, zinc chloride, zinc nitrate, zinc acetate, zinc perchlorate, zinc gluconate, zinc trifluoromethanesulfonate, and zinc bistrifluoromethanesulfonyl imide.
[0031] The technical solution of the present invention has the following advantages:
[0032] A. The present invention uses zinc oxide nanorods as templates, generates zinc sulfide-coated zinc oxide by surface sulfidation, and further performs chemical etching to remove the unreacted zinc oxide inside, thereby obtaining a hollow zinc sulfide nanotube material; the hollow zinc sulfide nanotube is then paired with a zinc metal negative electrode as a positive electrode material, and an aqueous electrolyte is injected to assemble an aqueous zinc-sulfur battery. The hollow zinc sulfide nanotube positive electrode material has excellent conductivity, can effectively improve the battery polarization phenomenon, and significantly improve the charge and discharge performance of the aqueous zinc-sulfur battery. The material provides sufficient buffer space for the volume change generated during the oxidation of sulfur, significantly reduces the damage to the electrode structure, and thus enhances the cycle stability of the battery.
[0033] B. In the preparation process, the present invention provides a variety of optional metal salts, alkali metal hydroxides, polyol solvents, etc., making the preparation process more flexible and controllable. The prepared hollow zinc sulfide nanotubes are not only suitable for the positive electrode of aqueous zinc-sulfur batteries, but their unique properties may also be extended to other related fields, and have wide application potential. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the specific embodiments of the present invention, the drawings required for use in the specific embodiments will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0035] Figure 1 (a) to (d) are scanning electron microscope images of hollow zinc sulfide nanotubes prepared from zinc oxide nanorods and thioacetamide in molar ratios of 1:1, 3:1, 6:1 and 12:1 in Example 1 of the present invention, respectively.
[0036] Figure 2 This is a test diagram of the cycle performance of a zinc-sulfur battery assembled with a hollow zinc sulfide cathode prepared with zinc oxide nanorods and thioacetamide in molar ratios of 1:1, 3:1, 6:1 and 12:1 as the positive electrode.
[0037] Figure 3 This is a rate performance test diagram of a zinc-sulfur battery assembled with a hollow zinc sulfide cathode prepared with zinc oxide nanorods and thioacetamide in molar ratios of 1:1, 3:1, 6:1 and 12:1 as the positive electrode. DETAILED DESCRIPTION
[0038] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] Embodiment 1:
[0040] This embodiment provides a method for preparing hollow zinc sulfide nanotubes for the positive electrode of an aqueous zinc-sulfur battery. The zinc-sulfur battery is mainly assembled from a hollow zinc sulfide nanotube material as a positive electrode, a zinc metal sheet as a negative electrode, a separator and an aqueous electrolyte.
[0041] The preparation method of the hollow zinc sulfide nanotube comprises the following steps:
[0042] S1. Preparation of zinc oxide nanorods: 0.015 mol of zinc acetate dihydrate was dissolved in 45 ml of an aqueous solution of 0.3 mol of sodium hydroxide, and 105 ml of propylene glycol was added after stirring evenly. The mixture was placed in a reactor for hydrothermal reaction at 160° C. for 20 h, and then washed, filtered, and dried to obtain zinc oxide nanorods.
[0043] S2, surface sulfurization: the zinc oxide nanorods and thioacetamide in step S1 are dissolved in a mixed solution of ethanol and water in a ratio of 1:3 at a molar ratio of 1:1, 3:1, 6:1 and 12:1, respectively, and then stirred at 80° C. for 3 h, and washed, filtered and dried to obtain a zinc sulfide-coated zinc oxide material;
[0044] S3, chemical etching: The zinc sulfide-coated zinc oxide materials prepared in the four ratios in step S2 were uniformly dispersed in 400 mL of 1.5 mol / L ammonium chloride aqueous solution, and then stirred for reaction at 80° C. for 6 h. After washing, filtering and drying, hollow zinc sulfide nanotube materials were obtained, such as Figure 1 As shown;
[0045] The following steps are for the application of hollow zinc sulfide nanotubes in zinc-sulfur batteries:
[0046] S4, mixing the hollow zinc sulfide material obtained in step S3 with conductive carbon black and a binder in a ratio of 7:2:1 to prepare a slurry, then coating the mixture on the surface of the current collector, and drying the mixture to obtain a positive electrode sheet for a zinc-sulfur battery;
[0047] S5. Assemble a zinc-sulfur battery by combining the positive electrode sheet obtained in step S4 with a zinc metal sheet, a separator and an aqueous electrolyte.
[0048] Figure 1 is a scanning electron microscope image of the hollow zinc sulfide nanotubes prepared in this embodiment. Figure 1(a), (b), (c), and (d) are hollow zinc sulfide nanotubes prepared by using zinc oxide nanorods and thioacetamide in molar ratios of 1:1, 3:1, 6:1, and 12:1, respectively. Figure 1 It can be seen that the hollow zinc sulfide nanotubes prepared are all tubular structures with zinc sulfide on the outside and no solid filling inside. The tube length is about 500nm to 3μm, and the tube mouth length is about 10nm to 500nm. Figure 1 It can be clearly observed that as the preparation ratio of zinc oxide nanorods and thioacetamide increases, the degree of damage of the prepared hollow zinc sulfide nanotubes gradually increases. This indicates that as the ratio of the two increases, the outer layer of zinc sulfide formed by the zinc sulfide-coated zinc oxide formed by the sulfidizing agent sulfidizing zinc oxide nanorods becomes thinner, and etching the zinc oxide inside with an etchant at the same temperature and for the same time will cause greater damage to the outer layer of zinc sulfide. The molecular structure of sulfur is stable, and electrons are bound around atoms. When the positive electrode material is zinc sulfide, the chemical bond changes from a covalent bond of sulfur to an ionic bond, which improves the conductivity. The hollow structure of the zinc sulfide of the present invention is also expected to optimize the ion transport path and accelerate the reaction kinetics. Figure 1 It can be seen that with the increase in the preparation ratio, the length of the hollow zinc sulfide gradually decreases, reducing the agglomeration of zinc sulfide and accelerating the reaction kinetics. However, due to the increase in the degree of damage, the hollow zinc sulfide nanotubes that were originally a whole long tube are dispersed into smaller hollow zinc sulfides. These damaged and miniaturized zinc sulfides agglomerate, which may also lead to slow kinetics. At the same time, the damage of the outer layer of zinc sulfide prepared in an appropriate proportion and the hollow structure of zinc sulfide can provide a certain space to alleviate the impact of the volume change of sulfur during the charging and discharging process. The electrode structure can be protected to a certain extent, improving the electrochemical activity of the positive electrode, thereby improving the cycle stability and life of the aqueous zinc-sulfur battery.
[0049] Figure 2 This is a test diagram of the cycle performance of a zinc-sulfur battery assembled with the hollow zinc sulfide prepared in this embodiment as the positive electrode; Figure 3 This is a rate performance test diagram of a zinc-sulfur battery assembled with hollow zinc sulfide prepared in this embodiment as the positive electrode. Figure 2 and Figure 3 It can be seen that the zinc-sulfur battery assembled with hollow zinc sulfide as the positive electrode has good cycle performance and rate performance, but the zinc-sulfur batteries assembled with hollow zinc sulfide as the positive electrode prepared in different ratios are also different. The hollow zinc sulfide prepared in the ratio of 3:1 and 6:1 has moderate thickness and damage, and the zinc sulfide aggregation is relatively smaller, which ensures that the assembled battery has good stability and rate performance. Figure 2It can be seen that the initial discharge capacity of zinc-sulfur batteries assembled with hollow zinc sulfide in four ratios as the positive electrode can reach as low as 324.9 mAh / g, and can be stably cycled for 400 cycles at 0.5 A / g, proving that the prepared hollow zinc sulfide can provide space for the volume change of sulfur during the charge and discharge process, thereby improving the life and stability of the battery. Figure 3 It can be seen that the rate performance of zinc-sulfur batteries assembled with hollow zinc sulfide prepared in a ratio of 1:1 and 12:1 as the positive electrode is poor. The hollow zinc sulfide nanotube structure prepared in a ratio of 1:1 is relatively complete, and the outer layer of zinc sulfide is thicker. In comparison, the zinc sulfide aggregation is more serious, which reduces the electrochemical activity. The hollow zinc sulfide prepared in a ratio of 12:1 is smaller in size and thickness, which shortens the migration path of ions and electrons and improves the reaction kinetics. However, due to the aggregation of these miniaturized zinc sulfides, the conductivity is reduced, resulting in insufficient kinetics, so the battery performance is worse at high rates.
[0050] In summary, hollow zinc sulfide nanotubes prepared by zinc oxide nanorods and thioacetamide in an appropriate molar ratio can well solve the pain point of volume change, while shortening the reaction path, improving conductivity, and alleviating the problem of insufficient kinetics.
[0051] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. However, the obvious changes or modifications derived therefrom are still within the scope of protection of the present invention.
Claims
1. A method for preparing hollow zinc sulfide nanotubes for positive electrodes of aqueous zinc-sulfur batteries, characterized in that: The following steps are involved: S1. Preparation of zinc oxide nanorods: 2+ The metal salt is dissolved in an aqueous solution of an alkali metal hydroxide, and after being stirred evenly, a polyol organic solvent is added in proportion, and the mixture is placed in a reactor for hydrothermal reaction to obtain zinc oxide nanorods; S2, surface vulcanization: dissolving the zinc oxide nanorods and the vulcanizing agent in the step S1 in a mixed solution of ethanol and water, and then stirring at a certain temperature to perform a vulcanization reaction to obtain a zinc sulfide-coated zinc oxide material; S3, chemical etching: the zinc sulfide-coated zinc oxide material in step S2 is uniformly dispersed in an etchant aqueous solution, and then stirred at a certain temperature to perform a chemical etching reaction to obtain a hollow zinc sulfide nanotube material.
2. The preparation method according to claim 1, characterized in that: The step S1 contains Zn 2+ The metal salt is at least one of zinc acetate dihydrate, zinc nitrate hexahydrate, zinc chloride, zinc nitrate and zinc sulfate; the Zn-containing 2+ The molar concentration of the metal salt is 0.1 to 0.5 mol / L; In step S1, the alkali metal hydroxide is at least one of lithium hydroxide, sodium hydroxide and potassium hydroxide; the molar concentration of the alkali metal hydroxide is 6 to 10 mol / L; In step S1, the polyol solvent is at least one of ethylene glycol, propylene glycol, and glycerol; the volume ratio between the polyol solvent and the aqueous solution is (2-5):1; The temperature of the hydrothermal reaction in step S1 is 120-180° C., and the reaction time is 12-24 hours.
3. The preparation method according to claim 1, characterized in that: In step S2, the vulcanizing agent is at least one of thioacetamide, thiourea and sodium sulfide; the molar ratio between the added zinc oxide nanorods and the vulcanizing agent is (1-12):1; The volume ratio of the mixed solution of ethanol and water in step S2 is 1:(2-4); The temperature of the sulfurization reaction in step S2 is 60-80° C., and the reaction time is 2-8 hours.
4. The preparation method according to claim 1, characterized in that: In step S3, the chemical etchant is at least one of ammonia water, ammonium chloride, sodium hydroxide and potassium hydroxide; the molar concentration of the etchant aqueous solution is 1 to 3 mol / L; The temperature of the chemical etching reaction in step S3 is 60-80° C., and the reaction time is 6-12 hours.
5. A hollow zinc sulfide nanotube for a positive electrode of an aqueous zinc-sulfur battery obtained by the preparation method according to any one of claims 1 to 4.
6. Use of the hollow zinc sulfide nanotubes prepared by the preparation method according to any one of claims 1 to 4 in aqueous zinc-sulfur batteries, characterized in that: The aqueous zinc-sulfur battery is assembled by using the hollow zinc sulfide nanotube as a positive electrode, a zinc metal sheet as a negative electrode, a separator and an aqueous electrolyte.
7. The use according to claim 6, characterized in that: The hollow zinc sulfide nanotubes are mixed with conductive carbon black and a binder in a certain proportion to prepare a slurry, which is then coated on the surface of a current collector and dried to obtain a positive electrode sheet for an aqueous zinc-sulfur battery; wherein the conductive carbon black is at least one of Super P, acetylene black, and Ketjen black; the binder is at least one of LA133, sodium alginate, PVDF, and PTFE; and the current collector is at least one of stainless steel foil, stainless steel mesh, titanium foil, titanium mesh, carbon fiber cloth, carbon paper, and graphite paper.
8. The use according to claim 7, characterized in that: The mass ratio of the hollow zinc sulfide nanotubes to the conductive carbon black and the binder is one of 9:0.5:0.5, 8:1:1, 7:2:1 and 6:3:
1.
9. The use according to claim 6, characterized in that: The diaphragm is at least one of glass fiber, non-woven fabric, and proton exchange membrane; The aqueous electrolyte is prepared by dissolving zinc metal salt in deionized water solution, and its concentration is 1-10 mol / L.
10. The use according to claim 9, characterized in that: The zinc metal salt is at least one of zinc sulfate, zinc chloride, zinc nitrate, zinc acetate, zinc perchlorate, zinc gluconate, zinc trifluoromethanesulfonate, and zinc bistrifluoromethanesulfonyl imide.
Citation Information
Patent Citations
Nano-zinc oxide with controllable length and preparation method thereof
CN104609460A
Preparation method of cathode materials for lithium ion batteries
CN109037642A
Molybdenum disulfide multistage double-layer hollow nanotube negative electrode material for zinc ion battery
CN115133001A
Zinc negative electrode and battery
JP2014167910A
Cited By
Tungsten carbide modified nitrogen-doped hollow rod-like carbon material as well as preparation method and application thereof
CN122426744A
Tungsten carbide modified nitrogen-doped hollow rod-like carbon material, and preparation method and application thereof