Room-temperature hydrogen sensing material with Pd-SnO2 (at) WO3 ternary core-shell structure and preparation method of room-temperature hydrogen sensing material
By designing the Pd-SnO2@WO3 ternary core-shell structure, using hydrothermal method to prepare SnO2 hollow spheres and loading WO3 and Pd particles, the problems of low selectivity and long response recovery time of existing SnO2-based hydrogen sensors are solved, and high efficiency is achieved The room temperature hydrogen sensing performance is suitable for hydrogen leakage monitoring.
Patent Information
- Application Number
- CN202410877759.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-11-22
AI Technical Summary
The existing SnO2-based hydrogen sensors have problems such as low selectivity and long response recovery time. The binary composite modification effect is limited, and it is necessary to further improve the hydrogen sensing performance.
A room temperature hydrogen sensing material with Pd-SnO2@WO3 ternary core-shell structure was designed, and SnO2 hollow spheres were prepared by hydrothermal method, and WO3 shell and Pd particles were uniformly loaded on its surface to form high oxygen vacancy and high redox Active ternary core-shell structure.
It realizes high sensitivity, short response recovery time and excellent selectivity of hydrogen sensing performance at room temperature, which is suitable for monitoring and early warning of hydrogen leakage, and the specific surface area and energy band structure of the material are significantly optimized.
Smart Images

Figure CN118993138A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of semiconductor gas sensors, and specifically relates to a Pd-SnO 2 @WO 3 A room temperature hydrogen sensing material with a ternary core-shell structure and a preparation method thereof. Background Art
[0002] Hydrogen is an industrial resource with broad application prospects. As a clean energy that can replace fossil fuels, hydrogen has gradually attracted attention in the industrial field. However, hydrogen is colorless, odorless, flammable and explosive, with an explosion range of 4%-75% in the air. In addition, due to the small molecules, low ignition energy (572kJ / mo), wide explosion limit and fast diffusion of hydrogen, it brings serious safety hazards to the promotion and application of hydrogen energy. Therefore, it is particularly important to carry out high-precision real-time (response recovery time <30s) room temperature (25℃) monitoring during the development, storage, transportation and use of hydrogen.
[0003] So far, various types of hydrogen sensors have been developed, including semiconductor, thermoelectric, optical and surface acoustic wave sensors. Among them, hydrogen sensors based on metal oxide semiconductor (MOS) have been widely studied and applied due to their low cost, high sensitivity and convenient operation. 2 , WO 3 , ZnO, TiO 2 etc. can be used as sensitive materials for hydrogen sensing. Among them, SnO 2 Due to its low work function, high carrier concentration and stable chemical properties, it is gradually used in hydrogen sensors. 2 The basic sensors usually face problems such as low selectivity, long response recovery time, and poor stability, which require further modification to improve the hydrogen sensing performance.
[0004] Currently, SnO 2 The modification mainly includes precious metal loading (Pd, Au) and compounds (ZnO, NiO, Co 3 O 4 ) composite, etc. Duan et al. synthesized SnO supported by Pd particles through a one-pot hydrothermal method. 2 hollow spheres, with a response of 14.5 to 200 ppm hydrogen at 330 °C (doi.org / 10.1016 / j.snb.2021.130557); Hu et al. prepared SnO by electrospinning 2-ZnO composite fiber, the response to 100 ppm hydrogen at 300 ° C is 18 (doi.org / 10.1016 / j.ceramint.2020.05.242). Since these modifications are mainly focused on binary composites, the improvement of hydrogen sensing performance is still limited.
[0005] Inspired by this, SnO 2 The basic ternary system helps to improve the dilemma. On the one hand, WO 3 As a unique hydrogen-induced color-changing material with high oxygen vacancies and hydrogen diffusion flux, it has attracted much attention in the field of optical hydrogen sensing. However, in resistive hydrogen sensors, especially when combined with tin oxide to form SnO 2 -WO 3 There are few studies on composite systems. For example, V.Ambardekar et al. used plasma spraying to coat WO 3 and SnO 2 The powder forms a nano-plate structure, and the response value to 500ppm hydrogen at 150℃ is 11 (SnO 2 :4.5), and the response recovery time is 35 / 269s (doi.org / 10.1016 / j.ijhydene.2022.03.005). On the other hand, precious metals have high work functions, reduce reaction energy and enhance chemical activity. Among them, Pd also has a unique sensitization reaction for hydrogen, including the formation of PdHX compounds and volume expansion effect. Therefore, Pd-SnO 2 -WO 3 Composite systems have great research prospects.
[0006] However, the current binary / ternary systems for hydrogen sensing materials include nanospheres, nanoblocks, nanofibers, nanowires, nanosheets, nanobelts and other structures. In order to further improve the Pd-SnO 2 -WO 3 The hydrogen sensing performance, microstructure, size and morphology of the ternary composite system also need to be carefully designed. The hollow spherical structure is currently less studied. It can adjust the size of the sphere and the thickness of the core-shell to make the material have a rich specific surface area, easy to modify, dense contact and not easy to agglomerate, and has great application prospects. In addition, optimizing the morphology and size of the spherical structure can also optimize the composite heterojunction and significantly increase the active reaction sites on the surface of the material, and adjust the ground state resistance of the material to achieve efficient room temperature hydrogen sensing. Summary of the invention
[0007] The present invention provides a Pd-SnO 2 @WO 3The room-temperature hydrogen sensing material with a ternary core-shell structure and its preparation method have high oxygen vacancies, high redox activity, optimized morphology and energy band structure. In terms of hydrogen detection, it has the advantages of room-temperature detection, high sensitivity, good selectivity and short response-recovery time, and can be used for monitoring and early warning of hydrogen leaks.
[0008] The technical solution of the present invention is as follows:
[0009] Pd-SnO 2 @WO 3 The room temperature hydrogen sensing material with a ternary core-shell structure is based on SnO 2 For the core, WO 3 Ternary core-shell hollow spheres loaded with Pd shell and Pd particles.
[0010] Furthermore, the Pd-SnO 2 @WO 3 Ternary core-shell structure room temperature hydrogen sensing material, in which SnO 2 Core and WO 3 The ratio of the amount of material of the shell is: n(SnO 2 ):n(WO 3 )=1:0.1~0.3,SnO 2 Core+WO 3 The mass ratio of SnO shell to Pd particle is: 2 @WO 3 ):m(Pd)=1:0.05~0.15.
[0011] Furthermore, the Pd-SnO 2 @WO 3 Ternary core-shell structure room temperature hydrogen sensing material, SnO 2 The diameter of the core is 130-150 nm, and the diameter of its inner cavity is 30-50 nm; WO 3 The thickness of the shell is 16-26 nm; the diameter of the Pd particles is 18-24 nm.
[0012] The above Pd-SnO 2 @WO 3 The method for preparing a room temperature hydrogen sensing material with a ternary core-shell structure comprises the following steps:
[0013] Step 1: Prepare tin tetrachloride hydrate (SnCl 4 ·5H 2 O) and hydrochloric acid solution are added to ethanol to form a mixture, and the mixture is transferred into an autoclave for hydrothermal reaction; after the autoclave is cooled to room temperature, centrifugal separation and washing are performed to obtain a precipitated product, and SnO is obtained after drying. 2 Precursor;
[0014] Step 2: SnO 2 The precursor is sintered in a muffle furnace to obtain SnO 2 Hollow sphere material;
[0015] Step 3: SnO 2 Hollow sphere material and sodium tungstate hydrate (Na 2 WO 4 ·2H 2 O) was added into deionized water and stirred at room temperature until uniform to obtain a mixed solution; concentrated sulfuric acid was slowly added dropwise to the mixed solution until it turned yellow, and the solid product after centrifugal separation was washed and dried to obtain SnO 2 @WO 3 Precursor;
[0016] Step 4: SnO 2 @WO 3 The precursor is sintered in a muffle furnace to obtain SnO 2 @WO 3 Core-shell hollow sphere materials;
[0017] Step 5: SnO 2 @WO 3 The core-shell hollow sphere material is placed in deionized water and palladium chloride is added, and stirred at room temperature to obtain a mixed solution; ascorbic acid is slowly added to the mixed solution and stirred continuously at room temperature, and a precipitate is obtained after centrifugation, and the precipitate is washed and dried to obtain Pd-SnO 2 @WO 3 Room temperature hydrogen sensing material with ternary core-shell structure.
[0018] Furthermore, in the preparation method, in step 1, SnCl 4 ·5H 2 The dosage of O is 185-195 mg, the concentration of the hydrochloric acid solution is 2 mol / L, and the ratio of the hydrochloric acid solution to anhydrous ethanol is 1:9-11; the temperature of the hydrothermal reaction is 170-180°C, and the hydrothermal reaction time is 24 hours; when centrifuging and washing, the anhydrous ethanol and deionized water are used for washing and centrifugation 2-3 times respectively to obtain a precipitated product; when the precipitated product is dried, it is placed in a vacuum oven at 60-80°C and dried for 12-24 hours.
[0019] Furthermore, in the preparation method, in step 2, the muffle furnace calcination temperature is 400° C., and the calcination time is 2 hours.
[0020] Furthermore, in the preparation method, in step 3, SnO 2 The amount of hollow sphere material is 1mmol, SnO 2 Hollow sphere material and Na 2 WO 4 ·2H2 The molar ratio of O is 1:0.1-0.3, the volume of deionized water is 40 mL; the concentration of concentrated sulfuric acid is 12 mol / L, and the volume of concentrated sulfuric acid added is 100-300 μL; during centrifugal separation, the product is washed and centrifuged with anhydrous ethanol and deionized water for 2-3 times respectively to obtain a solid product; when the solid product is dried, it is placed in a vacuum oven at 60-80° C. and dried for 12-24 hours.
[0021] Furthermore, in the preparation method, in step 4, the muffle furnace calcination temperature is 500° C., and the calcination time is 2 hours.
[0022] Furthermore, in the preparation method, in step 5, SnO 2 @WO 3 35-45 mg of core-shell hollow sphere material was used, the volume of deionized water was 20 mL, SnO 2 @WO 3 With PdCl 2 The mass ratio is 1:0.05-0.15; the amount of ascorbic acid added is 90-110 mg, and the stirring time is 20-24 hours; when centrifuging, wash and centrifuge with anhydrous ethanol and deionized water respectively for 2-3 times to obtain a precipitate; when the precipitate is dried, put it into a 60-80C vacuum oven and dry it for 12-24 hours.
[0023] The beneficial effects of the present invention are:
[0024] 1. The present invention designs Pd particles loaded with SnO by step-by-step modification. 2 @WO 3 Ternary core-shell hollow sphere gas sensing material, SnO 2 The hollow sphere has a suitable volume, WO 3 The core-shell is distinct and the thickness is reasonable. The Pd particles are evenly distributed and have a large specific surface area. The oxygen vacancies, hydrogen reaction activity, and carrier concentration of the material are improved, and the band structure is optimized. The hydrogen sensing test found that the optimal operating temperature of the material is reduced (260℃-180℃-60℃), among which 10Pd-SW-2 has the best sensing performance, and the sensing performance of 100ppm H at 25℃ is 100ppm. 2 The response value is 430, the response recovery time is 19 / 53s, the selectivity and anti-interference are also good, and the performance is excellent. It is helpful for efficient detection and early warning of hydrogen and is widely applicable.
[0025] 2. The present invention utilizes the different properties of material work functions and gradually optimizes the composition of the materials, constructs a ternary heterostructure, increases the specific surface area and redox activity, improves the energy band structure, realizes the ladder transmission of electrons, and improves the room temperature sensing performance of hydrogen. 2 -WO 3In the core-shell hollow sphere ternary composite system, due to the WO 3 The work function (4.9 eV) is smaller than that of SnO 2 (4.5 eV) is high, when it is uniformly loaded on spherical SnO 2 After the heterogeneous structure is formed on the surface, SnO 2 The free electrons are transferred to WO 3 This not only optimizes the band structure, but also allows more electrons on the surface of the composite system to be captured by adsorbed oxygen, thereby increasing the resistance of the sensing material in the air. The granular Pd has a higher work function (5.3 eV) and is loaded on SnO as a reactive site. 2 -WO 3 A more optimized ternary electron transport structure will be formed on the surface of the composite system.
[0026] 3. The preparation method of the present invention has the advantages of being simple and easy to operate, having a novel and controllable morphology, having low raw material cost, and being easy to realize large-scale production. It only requires two steps of hydrothermal and in-situ reduction, and is easy to realize large-scale production. It can also effectively adjust the SnO 2 The size of the hollow ball, WO 3 The thickness of the spherical shell is related to the size and dispersion of the Pd particles. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 is the temperature-response curve to 100 ppm hydrogen;
[0028] Figure 2 SnO in Comparative Example 1 2 Transmission electron microscope TEM image of hollow sphere;
[0029] Figure 3 TEM image of SW-1 in Comparative Example 3;
[0030] Figure 4 TEM image of SW-2 in Comparative Example 2;
[0031] Figure 5 TEM image of SW-3 in Comparative Example 4;
[0032] Figure 6 TEM image of 5Pd-SW-2 in Example 2;
[0033] Figure 7 TEM image of 10Pd-SW-2 in Example 1;
[0034] Figure 8 TEM image of 15Pd-SW-2 in Example 3;
[0035] Fig. 9 is the temperature-response curve to 100 ppm hydrogen;
[0036] Fig.10 The graph shows the response values of different gases at 100 ppm at 25°C. DETAILED DESCRIPTION
[0037] In order to more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings required for use in the embodiments or the prior art description are briefly introduced below, but the protection scope of the present invention is not limited to the following embodiments. It is clear to those skilled in the art that changes or adjustments can be made to the present invention without departing from the spirit and scope of the present invention, and these changes or adjustments are also included in the protection scope of the present invention.
[0038] Example 1
[0039] The Pd-SnO 2 @WO 3 The room temperature hydrogen sensing material with a ternary core-shell structure, the preparation method comprises the following steps:
[0040] S1. 0.19 g SnCl 4 ·5H 2 O and 30 mL of ethanol were added to 3 mL of 2M HCl solution; after stirring for 1 hour, the above solution was transferred to a stainless steel autoclave lined with polytetrafluoroethylene and heated at 180°C for 24 hours; after cooling to room temperature, it was washed three times with deionized water and ethanol to obtain a precipitate; the precipitate was dried at 60°C and calcined at 400°C for 2 hours to obtain SnO 2 Hollow ball;
[0041] S2. 1mmol SnO 2 Hollow spheres and 0.2mmol Na 2 WO 4 ·2H 2 O was dissolved in 40 mL of deionized water and 100-300 μL of 12 MH 2 SO 4 , until the white suspension turns yellow, the precipitate is washed with water and ethanol and dried at 60 °C; finally, the product is calcined at 500 °C for 2 h to obtain SnO 2 @WO 3 Core-shell hollow spheres;
[0042] S3. Add 40mg SnO 2 @WO 3 The core-shell hollow spheres and 100 mg ascorbic acid were dispersed in 20 mL of deionized water, and 4 mg of PdCl 2, stirred for 24 hours; the precipitate was washed and dried in air at 60°C for 12 hours. The product was recorded as 10Pd-SW-2; its transmission electron microscope TEM photo is shown as follows Figure 7 shown.
[0043] Example 2
[0044] The only difference between this embodiment and embodiment 1 is that the PdCl added in step S3 2 The amount of the substance is 2 mg, and the product is recorded as 5Pd-SW-2; its transmission electron microscope TEM photo is as follows Figure 6 shown.
[0045] Example 3
[0046] The only difference between this embodiment and embodiment 1 is that the PdCl added in step S3 2 The amount of the substance is 6 mg, and the product is recorded as 15Pd-SW-2; its transmission electron microscope TEM photo is as follows Figure 8 shown.
[0047] Comparative Example 1
[0048] The preparation method of hydrogen sensing material comprises the following steps: 0.19g SnCl 4 ·5H 2 O and 30 mL of ethanol were added to 3 mL of 2 M HCl solution; after stirring for 1 hour, the above solution was transferred to a stainless steel autoclave lined with polytetrafluoroethylene and heated at 180 ° C for 24 hours; after cooling to room temperature, it was washed three times with deionized water and ethanol to obtain a precipitate; finally, the precipitate was dried at 60 ° C and calcined at 400 ° C for 2 h to obtain SnO 2 Hollow sphere; its transmission electron microscope TEM photo is as follows Figure 2 shown.
[0049] Comparative Example 2
[0050] The method for preparing the hydrogen sensing material comprises the following steps:
[0051] S1. 0.19 g SnCl 4 ·5H 2 O and 30 mL of ethanol were added to 3 mL of 2M HCl solution. After stirring for 1 hour, the above solution was transferred to a stainless steel autoclave lined with polytetrafluoroethylene and heated at 180 ° C for 24 hours; after cooling to room temperature, it was washed three times with deionized water and ethanol to obtain a precipitate; finally, the precursor was dried at 60 ° C and calcined at 400 ° C for 2 h to obtain SnO 2 Hollow ball;
[0052] S2. 1mmol SnO 2Hollow spheres and 0.2mmol Na 2 WO 4 ·2H 2 O was dissolved in 40 mL of deionized water and 200 μL of 12 MH 2 SO 4 , until the white suspension turns yellow, the precipitate is washed with water and ethanol and dried at 60 °C; finally, the product is calcined at 500 °C for 2 h to obtain SnO 2 @WO 3 The core-shell hollow sphere, the product is denoted as SW-2; its transmission electron microscope TEM photo is shown in Figure 4 shown.
[0053] Comparative Example 3
[0054] The only difference between this comparative example and comparative example 2 is that the Na 2 WO 4 ·2H 2 The amount of O substance is 0.1mmol, and the product is recorded as SW-1; its transmission electron microscope TEM photo is as follows Figure 3 shown.
[0055] Comparative Example 4
[0056] The only difference between this comparative example and comparative example 2 is that the Na 2 WO 4 ·2H 2 The amount of O substance is 0.3 mmol, and the product is recorded as SW-3; its transmission electron microscope TEM photo is shown in Figure 5 shown.
[0057] like Figure 1 As shown, SnO 2 SnO in Comparative Example 1 2 Hollow sphere; the optimal working temperature of all materials is 180℃, which is lower than that of the original SnO 2 of 260℃; SW-2 showed the highest response (6.3) at 180℃.
[0058] like Fig. 9 As shown, SnO 2 The optimum temperatures of SnO, SW-2 and 10Pd-SW-2 are 260, 180 and 60℃ respectively; 10Pd-SW-2 shows a fairly high response (430) even at 25℃. 2 The high response of 10Pd-SW-2 (25 °C) means that this material is very suitable for room temperature sensing of H 2; All samples show a decrease in resistance with increasing temperature, which is due to the desorption of chemically adsorbed oxygen anions with increasing temperature due to diffusion.
[0059] like Fig.10 As shown, 10Pd-SW-2 has a 2 Sensitive; calculated SnO 2 , SW-2 and 10Pd-SW-2 R hydrogen / R ethanol (selectivity coefficient, 100 ppm) are 0.23, 0.26 and 10.75, respectively, indicating that 10Pd-SW-2 has excellent H 2 Selective.
Claims
1. Room temperature hydrogen sensing material with Pd-SnO2@WO3 ternary core-shell structure, characterized in that: Its structure is a ternary core-shell hollow sphere with SnO2 as core, WO3 as shell and Pd particles as load.
2. The room temperature hydrogen sensing material of the Pd-SnO2@WO3 ternary core-shell structure according to claim 1, characterized in that: The amount ratio of SnO2 core to WO3 shell is: n(SnO2):n(WO3)=1:0.1~0.3, and the mass ratio of SnO2 core+WO3 shell to Pd particles is: m(SnO2@WO3):m(Pd)=1:0.05~0.
15.
3. The room temperature hydrogen sensing material of the Pd-SnO2@WO3 ternary core-shell structure according to claim 1, characterized in that: The diameter of the SnO2 core is 130-150nm, and the diameter of its inner cavity is 30-50nm; the thickness of the WO3 shell is 16-26nm; and the diameter of the Pd particle is 18-24nm.
4. The method for preparing the room temperature hydrogen sensing material of the Pd-SnO2@WO3 ternary core-shell structure according to any one of claims 1 to 3, characterized in that: The following steps are involved: Step 1: adding tin tetrachloride hydrate (SnCl4·5H2O) and hydrochloric acid solution to ethanol to form a mixture, and transferring the mixture into an autoclave for hydrothermal reaction; cooling the autoclave to room temperature, centrifuging and washing, obtaining a precipitated product, and drying to obtain a SnO2 precursor; Step 2: placing the SnO2 precursor in a muffle furnace for sintering to obtain a SnO2 hollow sphere material; Step 3: Add the SnO2 hollow sphere material and sodium tungstate hydrate (Na2WO4·2H2O) to deionized water, stir at room temperature until uniform, and obtain a mixed solution; add concentrated sulfuric acid dropwise and slowly to the mixed solution until it turns yellow, wash the solid product after centrifugation, and dry it to obtain a SnO2@WO3 precursor; Step 4: sintering the SnO2@WO3 precursor in a muffle furnace to obtain a SnO2@WO3 core-shell hollow sphere material; Step 5: Place the SnO2@WO3 core-shell hollow sphere material in deionized water and add palladium chloride, stir evenly at room temperature to obtain a mixed solution; slowly add ascorbic acid to the mixed solution and continue stirring at room temperature, obtain a precipitate after centrifugation, wash and dry, and obtain a room temperature hydrogen sensing material with a Pd-SnO2@WO3 ternary core-shell structure.
5. The preparation method according to claim 4, characterized in that: In the step 1, the amount of SnCl4·5H2O is 185-195 mg, the concentration of the hydrochloric acid solution is 2 mol / L, and the ratio of the hydrochloric acid solution to anhydrous ethanol is 1:9-11; the temperature of the hydrothermal reaction is 170-180°C, and the hydrothermal reaction time is 24 hours; during centrifugal separation and washing, the product is washed and centrifuged 2-3 times with anhydrous ethanol and deionized water respectively to obtain a precipitated product; when the precipitated product is dried, it is placed in a vacuum oven at 60-80°C and dried for 12-24 hours.
6. The preparation method according to claim 4, characterized in that: In the step 2, the calcination temperature in the muffle furnace is 400° C., and the calcination time is 2 hours.
7. The preparation method according to claim 4, characterized in that: In the step 3, the amount of SnO2 hollow sphere material is 1 mmol, the molar ratio of SnO2 hollow sphere material to Na2WO4·2H2O is 1:0.1-0.3, and the volume of deionized water is 40 mL; the concentration of concentrated sulfuric acid is 12 mol / L, and the volume of concentrated sulfuric acid added is 100-300 μL; during centrifugal separation, the product is washed and centrifuged with anhydrous ethanol and deionized water for 2-3 times respectively to obtain a solid product; when the solid product is dried, it is placed in a vacuum oven at 60-80°C and dried for 12-24 hours.
8. The preparation method according to claim 4, characterized in that: In the step 4, the calcination temperature in the muffle furnace is 500° C. and the calcination time is 2 hours.
9. The preparation method according to claim 4, characterized in that: In the step 5, 35-45 mg of SnO2@WO3 core-shell hollow sphere material is taken, the volume of the deionized water is 20 mL, the mass ratio of SnO2@WO3 to PdCl2 is 1:0.05-0.15; the amount of ascorbic acid added is 90-110 mg, and the stirring time is 20-24 hours; during centrifugation, the precipitate is washed and centrifuged with anhydrous ethanol and deionized water for 2-3 times respectively to obtain a precipitate; when the precipitate is dried, it is placed in a 60-80°C vacuum oven and dried for 12-24 hours.