Low-hysteresis high-dielectric adjustable ferroelectric material and preparation method and application thereof

By introducing Bi3+ ions and low melting point bismuth nitrate into barium strontium titanate, the dielectric constant and hysteresis problems of existing ferroelectric materials were solved, and low hysteresis and high dielectric adjustable ferroelectric materials were prepared, achieving dielectric performance The stability and moderate dielectric constant are suitable for applications such as ferroelectric phase shifters.

CN118993143APending Publication Date: 2024-11-22XIDIAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411078324.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The dielectric constant and dielectric loss of existing high-dielectric adjustable ferroelectric materials are relatively large, which is difficult to meet the impedance matching requirements. In addition, there is a significant hysteresis phenomenon in the dielectric constant and polarization strength, which limits the high-performance ferroelectric shift. The development of the phase device.

Method used

A-position non-equivalent replacement is performed by introducing Bi3+ ions in barium strontium titanate (Sr0.6Ba0.4TiO3), and bismuth nitrate with a low melting point under the condition of a preparation temperature below 700°C, low hysteresis high is prepared. Dielectrically adjustable ferroelectric materials to increase their polarization strength and dielectric constant.

Benefits of technology

A ferroelectric material with a dielectric constant stable in the temperature range of 25 to 300°C and an almost unchanged dielectric tuning rate in the range of 1 to 100 kHz has excellent temperature and frequency stability, and is suitable for ferroelectric phase shifters. Ferroelectric adjustable filter and variable capacitor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993143A_ABST
    Figure CN118993143A_ABST
Patent Text Reader

Abstract

The invention discloses a low-hysteresis high-dielectric adjustable ferroelectric material and a preparation method and application thereof, the chemical general formula of the ferroelectric material is (Sr0. 6Ba0. 4) (1-1.5 x) BixTiO3, and x is more than 0 and less than 0.4; according to the method, Bi < 3 + > ions are used for carrying out non-equivalent replacement on the A site of barium strontium titanate (Sr0. 6Ba0. 4TiO3) in a paraelectric phase at room temperature, orbital hybridization can be generated between Bi and O, and the A site non-equivalent replacement can promote formation of a charged point defect, so that the polarization intensity and the dielectric constant of the ferroelectric material are improved; by introducing bismuth nitrate with a low melting point, the ferroelectric material with low loss, low hysteresis, moderate dielectric constant and excellent dielectric tuning characteristic can be obtained on the premise that the preparation temperature is lower than 700 DEG C, and the ferroelectric material can be widely applied to ferroelectric phase shifters, ferroelectric tunable filters, variable capacitors and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ferroelectric materials, and in particular relates to a low hysteresis high dielectric adjustable ferroelectric material and a preparation method and application thereof. Background Art

[0002] Phased array technology combines the characteristics of multi-beam shaping, fast scanning, anti-interference, and low weight, and has revolutionary significance for radar, satellite communications and other fields. However, as one of the most widely used pre-processing devices in phased arrays, phase shifters have become the key to restricting the development of phased array technology. Compared with existing ferrite phase shifters and semiconductor diode phase shifters, ferroelectric phase shifters developed based on the characteristic that the dielectric constant of ferroelectric materials changes with the applied bias electric field have many advantages such as simple structure, fast response speed, and good temperature stability. They are expected to lead the development direction of future phased array phase shifters. However, the dielectric constant and dielectric loss of existing high-dielectric adjustable ferroelectric materials are generally too large to meet the impedance matching requirements, and there is a significant hysteresis phenomenon in the dielectric constant and polarization intensity, which makes the development of high-performance ferroelectric phase shifters face huge challenges.

[0003] Based on the complete solid solution characteristics of perovskite-type barium titanate ferroelectric and perovskite-type strontium titanate paraelectric, the dielectric constant and Curie temperature of the obtained barium strontium titanate ferroelectric are easy to adjust. 1-x Sr x TiO3 multilayer tunable capacitors.Journal of the European Ceramic Society 41(2021)2559-2567.) studied Ba 1-x Sr xThe microstructure and dielectric properties of TiO3 multilayer tunable capacitors are studied by adjusting the ratio of Sr and Ba elements in strontium barium titanate ferroelectric materials to change the Curie temperature, thereby regulating its dielectric constant and dielectric tuning performance. However, the prepared bulk ceramics have problems such as large size, high preparation temperature, and poor semiconductor process integration. Xianxin Zhang et al. (Xianxin Zhang, Le Xin, Mingwei Zhang, Jiwei Zhai, Study on the intrinsic correlation between sintering method, ion diffusion, and dielectric properties of Ba 0.5 Sr 0.5 TiO3-ZnAl2O4 composite ceramics, Crystal Research And Technology 58 (2023) 2200235.) studied Ba 0.5 Sr 0.5 The intrinsic correlation among sintering method, ion diffusion and dielectric properties of TiO3-ZnAl2O4 composite ceramics was studied by 0.5 Sr 0.5 ZnAl2O4 was introduced into TiO3, and samples were prepared by solid phase sintering and microwave sintering. It was shown that microwave sintering could reduce the sintering temperature and refine the grain size. When the ZnAl2O4 content was 50wt%, a dielectric tuning rate of 40.03% could be achieved, but the preparation temperature was as high as 1300℃ or above; Wenlong Liu et al. (Wenlong Liu, Lin Tao, Wei Feng, Jiaxuan Liao, Lingzhao Zhang, Sandwich-type composite multilayer films of strontium titanate and barium strontiumtitanate and their controllabledielectric properties, Journal of Materials Science & Technology 85(2021)245-254.) proposed a multilayer composite film of strontium titanate and barium strontium titanate and studied its dielectric properties. A sandwich-type multilayer film consisting of strontium titanate and barium strontium titanate-based dielectric layers was prepared by a solution method. A dielectric tuning rate of 32.7% was obtained at 100 kHz, but the dielectric tuning rate decreased significantly with the increase of the thickness of the strontium titanate dielectric layer, and the hysteresis phenomenon of its electrical properties under an external electric field has not yet been paid attention to. Summary of the invention

[0004] In order to overcome the above-mentioned shortcomings of the prior art, the purpose of the present invention is to provide a low hysteresis high dielectric tunable ferroelectric material and its preparation method and application. 3+ Ion pairs of barium strontium titanate (Sr 0.6 Ba 0.4 By introducing bismuth nitrate with a low melting point, ferroelectric materials with low loss, low hysteresis, suitable dielectric constant and excellent dielectric tuning properties can be obtained under the premise of a preparation temperature below 700°C, which can be widely used in ferroelectric phase shifters, ferroelectric tunable filters and variable capacitors.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0006] A low hysteresis high dielectric tunable ferroelectric material, the chemical formula of the ferroelectric material is (Sr 0.6 Ba 0.4 ) (1-1.5x) Bi x TiO3, where 0<x<0.4.

[0007] Preferably, the value of x is: 0.05≤x≤0.3.

[0008] The ferroelectric material is a thin film material with a thickness of 200-400 nm.

[0009] The ferroelectric material is a perovskite structure and has defect dipole characteristics.

[0010] A method for preparing the low hysteresis high dielectric tunable ferroelectric material as described above comprises the following steps:

[0011] Step 1: According to the chemical formula (Sr 0.6 Ba 0.4 ) (1-1.5x) Bi x Barium acetate, strontium acetate and bismuth nitrate are weighed in the stoichiometric ratio of each element in TiO3 to obtain a mixed raw material; the mixed raw material is dissolved in a mixed solution of ethylene glycol methyl ether, acetic acid and ammonia water, and heated and stirred at 40 to 60° C. for 4 to 6 hours to obtain a solution A;

[0012] Step 2: According to the chemical formula (Sr 0.6 Ba 0.4 ) (1-1.5x) Bi xThe stoichiometric ratio of the Ti element in TiO3 was adjusted. Tetrabutyl titanate solution was weighed and mixed with acetylacetone solution and stirred for 4 to 6 hours to obtain solution B.

[0013] Step 3: Mix solution A and solution B, stir, and age for 20 to 35 hours to obtain (Sr) with a molar concentration of 0.2 to 0.3 mol / L. 0.6 Ba 0.4 ) (1-1.5x) Bi x TiO3 precursor solution;

[0014] Step 4: Spin-coat the precursor solution obtained in step 3 onto the pretreated substrate, then perform annealing and crystallization in a rapid annealing furnace, and repeat the spin-coating and annealing operation until a film with a thickness of 200 to 400 nm is obtained, i.e., a low hysteresis and high dielectric tunable ferroelectric material.

[0015] In the step 1, the volume ratio of ethylene glycol methyl ether: acetic acid: ammonia water is (5-6): (5-6): (0.5-1).

[0016] In the step 2, the volume ratio of tetrabutyl titanate solution to acetylacetone solution is (4-5):1.

[0017] The specific process of spin coating annealing in step 4 is as follows:

[0018] 1) dropping the precursor solution onto the substrate for spin coating, first rotating at a speed of 500 to 800 rpm for 5 to 10 seconds, and then rotating at a speed of 3000 to 4000 rpm for 25 to 35 seconds to obtain a spin-coated film;

[0019] 2) placing the spin-coated film obtained in step 1) in a rapid annealing furnace and annealing at 300-350° C. for 3-5 min, and then annealing at 560-650° C. for 5-10 min;

[0020] 3) Repeat step 1) and step 2) until a film with a thickness of 200-400 nm is obtained, that is, a low hysteresis and high dielectric tunable ferroelectric material.

[0021] The pretreatment process of the substrate in step 4 is: the substrate is cleaned in an ultrasonic cleaning machine using acetone, ethanol and distilled water in sequence for 5-15 minutes, and after cleaning, the substrate is blown dry using high-purity nitrogen.

[0022] Application of the low hysteresis and high dielectric tunable ferroelectric material or the low hysteresis and high dielectric tunable ferroelectric material prepared by the above preparation method in ferroelectric phase shifters or dielectric tunable capacitors.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. When Sr:Ba=3:2 in the low hysteresis high dielectric tunable ferroelectric material, it is in the paraelectric phase at room temperature. 3+ Ion pairs of barium strontium titanate (Sr 0.6 Ba 0.4 The A-site of TiO3) is subjected to non-equivalent substitution. Since orbital hybridization will occur between Bi and O, and the non-equivalent substitution at the A-site will promote the formation of charged point defects, the polarization strength and dielectric constant of the ferroelectric material are improved.

[0025] 2. The present invention introduces bismuth nitrate with a low melting point to prepare a ferroelectric film, which can obtain a ferroelectric material with low hysteresis and high dielectric tuning characteristics under annealing conditions below 700°C, and has simple chemical composition and preparation process. The dielectric constant can be maintained between 220 and 310 in the temperature range of 25 to 300°C, and the dielectric tuning rate hardly changes in the range of 1 to 100 kHz. The dielectric properties show excellent temperature stability and frequency stability.

[0026] To sum up, compared with the prior art, the low hysteresis and high dielectric tunable ferroelectric material prepared by the present invention has defect dipole characteristics, which greatly improves the polarization strength and dielectric constant of the ferroelectric material; by introducing bismuth nitrate with a low melting point, a ferroelectric material with low loss, low hysteresis, suitable dielectric constant and excellent dielectric tuning characteristics can be obtained under the premise that the preparation temperature is lower than 700°C, which can be widely used in ferroelectric phase shifters, ferroelectric tunable filters and variable capacitors, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is the XRD pattern of the low hysteresis and high dielectric tunable ferroelectric material provided in Example 1.

[0028] Figure 2 The hysteresis loop of the low hysteresis and high dielectric tunable ferroelectric material provided in Example 1.

[0029] Figure 3 This is a curve showing the change of the dielectric constant of the low hysteresis and high dielectric tunable ferroelectric material provided in Example 1 with temperature.

[0030] Figure 4 The dielectric constant change rate of the low hysteresis high dielectric tunable ferroelectric material provided in Example 1 within a temperature range of 25 to 300° C. and a frequency range of 1 to 100 kHz.

[0031] Figure 5 This is a curve showing the change of dielectric loss with temperature for the low hysteresis and high dielectric tunable ferroelectric material provided in Example 1.

[0032] Figure 6 This is a curve showing the change of the dielectric constant of the low hysteresis and high dielectric tunable ferroelectric material provided in Example 1 with the bias voltage.

[0033] Figure 7 The dielectric tuning rate of the low hysteresis and high dielectric tunable ferroelectric material provided in Example 1, wherein: Figure 7 (a) is 1kHz, Figure 7 (b) is 10kHz, Figure 7 (c) is 100kHz. DETAILED DESCRIPTION

[0034] The technical solution of the present invention is further introduced below in conjunction with the accompanying drawings and specific embodiments.

[0035] A low hysteresis high dielectric tunable ferroelectric material, the chemical formula of the ferroelectric material is (Sr 0.6 Ba 0.4 ) (1-1.5x) Bi x TiO3, wherein 0<x<0.4; the ferroelectric material is a thin film material with a thickness of 200~400nm; the (Sr 0.6 Ba 0.4 ) (1-1.5x) Bi x TiO3 thin film material has a perovskite structure.

[0036] When Sr:Ba=3:2 in the low hysteresis high dielectric tunable ferroelectric material, it is in the paraelectric phase at room temperature. The high-valent and low-melting-point bismuth element is used to partially non-equivalently replace the A position of the perovskite-type strontium barium titanate ferroelectric film, and no second phase is formed. The preparation temperature can be reduced while maintaining low dielectric loss. Since orbital hybridization occurs between Bi and O, the defect dipole formed can promote the improvement of polarization strength and dielectric constant.

[0037] A method for preparing a low hysteresis high dielectric tunable ferroelectric material comprises the following steps:

[0038] Step 1: According to the chemical formula (Sr 0.6 Ba 0.4 ) (1-1.5x) Bi x Barium acetate, strontium acetate and bismuth nitrate are weighed in the stoichiometric ratio of each element in TiO3 to obtain a mixed raw material; the mixed raw material is dissolved in a mixed solution of ethylene glycol methyl ether, acetic acid and ammonia water, and heated and stirred at 40-60°C for 4-6 hours to obtain a solution A; wherein, by volume ratio, ethylene glycol methyl ether: acetic acid: ammonia water = (5-6): (5-6): (0.5-1);

[0039] Step 2: According to the chemical formula (Sr 0.6 Ba 0.4 ) (1-1.5x) Bi xThe stoichiometric ratio of the Ti element in TiO3 is as follows: Weigh the tetrabutyl titanate solution, mix it with the acetylacetone solution, and stir it for 4 to 6 hours to obtain a solution B; by volume ratio, the tetrabutyl titanate solution: acetylacetone solution = (4 to 5): 1;

[0040] Step 3: Mix solution A and solution B, stir, and age for 20 to 35 hours to obtain (Sr) with a molar concentration of 0.2 to 0.3 mol / L. 0.6 Ba 0.4 ) (1-1.5x) Bi x TiO3 precursor solution;

[0041] Step 4: Spin-coat the precursor solution obtained in step 3 on the pretreated substrate, and then anneal and crystallize it in a rapid annealing furnace, and repeat the spin-coating annealing operation until a film with a thickness of 200 to 400 nm is obtained, that is, a low hysteresis and high dielectric tunable ferroelectric material;

[0042] The pretreatment process of the substrate is: the substrate is cleaned in an ultrasonic cleaning machine using acetone, ethanol and distilled water in sequence for 5-15 minutes, and after cleaning, the substrate is blown dry using high-purity nitrogen;

[0043] The specific process of the spin coating annealing is as follows:

[0044] 1) dropping the precursor solution onto the substrate for spin coating, first rotating at a speed of 500 to 800 rpm for 5 to 10 seconds, and then rotating at a speed of 3000 to 4000 rpm for 25 to 35 seconds to obtain a spin-coated film;

[0045] 2) placing the spin-coated film obtained in step 1) in a rapid annealing furnace and annealing at 300-350° C. for 3-5 min, and then annealing at 560-650° C. for 5-10 min;

[0046] 3) Repeat step 1) and step 2) until a film with a thickness of 200-400 nm is obtained, that is, a low hysteresis and high dielectric tunable ferroelectric material.

[0047] The low hysteresis and high dielectric adjustable ferroelectric material prepared by the present invention can be applied in the fields of dielectric adjustable capacitors or ferroelectric phase shifters; a Pt layer with a thickness of 100 to 200 nm is plated on the surface of the substrate, and an electrode with a diameter of 0.2 mm is plated on the surface of the low hysteresis and high dielectric adjustable ferroelectric material obtained in step 4 using a sputtering instrument to perform electrical performance testing.

[0048] Example 1

[0049] A low hysteresis high dielectric tunable ferroelectric material, the chemical formula of which is Sr 0.51 Ba 0.34 Bi 0.1TiO3; the ferroelectric material is a thin film material with a thickness of 380nm.

[0050] A method for preparing a low hysteresis high dielectric tunable ferroelectric material comprises the following steps:

[0051] Step 1: According to the chemical formula Sr 0.51 Ba 0.34 Bi 0.1 Barium acetate, strontium acetate and bismuth nitrate are weighed according to the stoichiometric ratio of each element in TiO3 to obtain a mixed raw material; the mixed raw material is dissolved in a mixed solution of ethylene glycol methyl ether, acetic acid and ammonia water, and heated and stirred at 40°C for 4 hours to obtain solution A; wherein the volume ratio of ethylene glycol methyl ether, acetic acid and ammonia water is 5:5:0.5;

[0052] Step 2: According to the chemical formula Sr 0.51 Ba 0.34 Bi 0.1 The stoichiometric ratio of the Ti element in TiO3 was 5:1. The tetrabutyl titanate solution was weighed and mixed with the acetylacetone solution and stirred for 6 hours to obtain a solution B.

[0053] Step 3: Mix solution A and solution B, stir, and age for 20 hours to obtain Sr with a molar concentration of 0.3 mol / L. 0.51 Ba 0.34 Bi 0.1 TiO3 precursor solution;

[0054] Step 4: Clean the substrate in an ultrasonic cleaner with acetone, ethanol and distilled water in turn for 5 minutes. After cleaning, blow dry the substrate with high-purity nitrogen; spin-coat the precursor solution obtained in step 3 on the substrate, first at a rotation speed of 500 rpm for 5 seconds, and then at a rotation speed of 3000 rpm for 35 seconds to obtain a spin-coated film; place the spin-coated film in a rapid annealing furnace and anneal at 350°C for 3 minutes, and then anneal at 600°C for 5 minutes; repeat the spin coating annealing operation until a film with a thickness of 380 nm is obtained, that is, a low hysteresis and high dielectric tunable ferroelectric material.

[0055] Example 2

[0056] A low hysteresis high dielectric tunable ferroelectric material, the chemical formula of which is Sr 0.42 Ba 0.28 Bi 0.2 TiO3; the ferroelectric material is a thin film material with a thickness of 380nm.

[0057] A method for preparing a low hysteresis high dielectric tunable ferroelectric material comprises the following steps:

[0058] Step 1: According to the chemical formula Sr0.42 Ba 0.28 Bi 0.2 Barium acetate, strontium acetate and bismuth nitrate are weighed according to the stoichiometric ratio of each element in TiO3 to obtain a mixed raw material; the mixed raw material is dissolved in a mixed solution of ethylene glycol methyl ether, acetic acid and ammonia water, and heated and stirred at 50°C for 6 hours to obtain a solution A; wherein the volume ratio of ethylene glycol methyl ether, acetic acid and ammonia water is 6:6:0.5;

[0059] Step 2: According to the chemical formula Sr 0.42 Ba 0.28 Bi 0.2 The stoichiometric ratio of the Ti element in TiO3 was 4:1. The tetrabutyl titanate solution was weighed and mixed with the acetylacetone solution and stirred for 5 hours to obtain a solution B. The volume ratio of the tetrabutyl titanate solution to the acetylacetone solution was 4:1.

[0060] Step 3: Mix solution A and solution B, stir, and age for 24 hours to obtain Sr with a molar concentration of 0.3 mol / L. 0.42 Ba 0.28 Bi 0.2 TiO3 precursor solution;

[0061] Step 4: Clean the substrate in an ultrasonic cleaner with acetone, ethanol and distilled water in turn for 10 minutes. After cleaning, blow dry the substrate with high-purity nitrogen; spin-coat the precursor solution obtained in step 3 on the substrate, first at a speed of 800 rpm for 5 seconds, and then at a speed of 3500 rpm for 35 seconds to obtain a spin-coated film; place the spin-coated film in a rapid annealing furnace and anneal at 300°C for 5 minutes, and then anneal at 620°C for 5 minutes; repeat the spin coating annealing operation until a film with a thickness of 380 nm is obtained, that is, a low hysteresis and high dielectric tunable ferroelectric material.

[0062] Example 3

[0063] A low hysteresis high dielectric tunable ferroelectric material, the chemical formula of which is Sr 0.33 Ba 0.22 Bi 0.3 TiO3; the ferroelectric material is a thin film material with a thickness of 350nm.

[0064] A method for preparing a low hysteresis high dielectric tunable ferroelectric material comprises the following steps:

[0065] Step 1: According to the chemical formula Sr 0.33 Ba 0.22 Bi 0.3Barium acetate, strontium acetate and bismuth nitrate are weighed according to the stoichiometric ratio of each element in TiO3 to obtain a mixed raw material; the mixed raw material is dissolved in a mixed solution of ethylene glycol methyl ether, acetic acid and ammonia water, and heated and stirred at 60°C for 4 hours to obtain a solution A; wherein the volume ratio of ethylene glycol methyl ether, acetic acid and ammonia water is 5:6:1;

[0066] Step 2: According to the chemical formula Sr 0.33 Ba 0.22 Bi 0.3 The stoichiometric ratio of the Ti element in TiO3 was 4.5:1. The tetrabutyl titanate solution was weighed and mixed with the acetylacetone solution and stirred for 6 hours to obtain a solution B.

[0067] Step 3: Mix solution A and solution B, stir, and age for 30 hours to obtain Sr with a molar concentration of 0.3 mol / L. 0.33 Ba 0.22 Bi 0.3 TiO3 precursor solution;

[0068] Step 4: Clean the substrate in an ultrasonic cleaner with acetone, ethanol and distilled water in turn for 15 minutes. After cleaning, blow dry the substrate with high-purity nitrogen; spin-coat the precursor solution obtained in step 3 on the substrate, first at a rotation speed of 600 rpm for 10 seconds, and then at a rotation speed of 4000 rpm for 35 seconds to obtain a spin-coated film; place the spin-coated film in a rapid annealing furnace and anneal at 300°C for 4 minutes, and then anneal at 560°C for 6 minutes; repeat the spin coating annealing operation until a film with a thickness of 350 nm is obtained, that is, a low hysteresis and high dielectric tunable ferroelectric material.

[0069] Example 4

[0070] A low hysteresis high dielectric tunable ferroelectric material, the chemical formula of which is Sr 0.555 Ba 0.37 Bi 0.05 TiO3; the ferroelectric material is a thin film material with a thickness of 200nm.

[0071] A method for preparing a low hysteresis high dielectric tunable ferroelectric material comprises the following steps:

[0072] Step 1: According to the chemical formula Sr 0.555 Ba 0.37 Bi 0.05 Barium acetate, strontium acetate and bismuth nitrate are weighed according to the stoichiometric ratio of each element in TiO3 to obtain a mixed raw material; the mixed raw material is dissolved in a mixed solution of ethylene glycol methyl ether, acetic acid and ammonia water, and heated and stirred at 60°C for 6 hours to obtain solution A; wherein the volume ratio of ethylene glycol methyl ether, acetic acid and ammonia water is 6:5:0.5;

[0073] Step 2: According to the chemical formula Sr 0.555 Ba 0.37 Bi 0.05 The stoichiometric ratio of the Ti element in TiO3 was 5:1. The tetrabutyl titanate solution was weighed and mixed with the acetylacetone solution and stirred for 4 hours to obtain a solution B.

[0074] Step 3: Mix solution A and solution B, stir, and age for 35 hours to obtain Sr with a molar concentration of 0.2 mol / L. 0.555 Ba 0.37 Bi 0.05 TiO3 precursor solution;

[0075] Step 4: Clean the substrate in an ultrasonic cleaner with acetone, ethanol and distilled water in turn for 10 minutes. After cleaning, blow dry the substrate with high-purity nitrogen; spin-coat the precursor solution obtained in step 3 on the substrate, first at a speed of 800 rpm for 8 seconds, and then at a speed of 3000 rpm for 25 seconds to obtain a spin-coated film; place the spin-coated film in a rapid annealing furnace and anneal at 350°C for 3 minutes, and then anneal at 650°C for 10 minutes; repeat the spin coating annealing operation until a film with a thickness of 200 nm is obtained, that is, a low hysteresis and high dielectric tunable ferroelectric material.

[0076] Example 5

[0077] A low hysteresis high dielectric adjustable ferroelectric material and a preparation method thereof, wherein the chemical formula of the ferroelectric material is Sr 0.465 Ba 0.31 Bi 0.15 TiO3; the ferroelectric material is a thin film material with a thickness of 400nm.

[0078] A method for preparing a low hysteresis high dielectric tunable ferroelectric material comprises the following steps:

[0079] Step 1: According to the chemical formula Sr 0.465 Ba 0.31 Bi 0.15 Barium acetate, strontium acetate and bismuth nitrate are weighed according to the stoichiometric ratio of each element in TiO3 to obtain a mixed raw material; the mixed raw material is dissolved in a mixed solution of ethylene glycol methyl ether, acetic acid and ammonia water, and heated and stirred at 50°C for 4 hours to obtain solution A; wherein the volume ratio of ethylene glycol methyl ether, acetic acid and ammonia water is 6:5:0.8;

[0080] Step 2: According to the chemical formula Sr 0.465 Ba 0.31 Bi 0.15The stoichiometric ratio of the Ti element in TiO3 was 4.8:1. The tetrabutyl titanate solution was weighed and mixed with the acetylacetone solution and stirred for 5 hours to obtain a solution B.

[0081] Step 3: Mix solution A and solution B, stir, and age for 20 hours to obtain Sr with a molar concentration of 0.25 mol / L. 0.465 Ba 0.31 Bi 0.15 TiO3 precursor solution;

[0082] Step 4: Clean the substrate in an ultrasonic cleaner with acetone, ethanol and distilled water in turn for 5 minutes. After cleaning, blow dry the substrate with high-purity nitrogen; spin-coat the precursor solution obtained in step 3 on the substrate, first at a rotation speed of 500 rpm for 10 seconds, and then at a rotation speed of 3500 rpm for 30 seconds to obtain a spin-coated film; place the spin-coated film in a rapid annealing furnace and anneal at 330°C for 4 minutes, and then anneal at 620°C for 8 minutes; repeat the spin coating annealing operation until a film with a thickness of 400 nm is obtained, that is, a low hysteresis and high dielectric tunable ferroelectric material.

[0083] The surface of the low hysteresis and high dielectric constant tunable ferroelectric material obtained in step 4 was plated with an electrode with a diameter of 0.2 mm using a sputtering apparatus for electrical performance testing. Figure 1 is the X-ray diffraction pattern of the low hysteresis high dielectric tunable ferroelectric material of Example 1, from Figure 1 It can be observed that the ferroelectric material prepared by the present invention has obvious (100), (110), (111), (200), and (211) diffraction peaks, and no impurity phase appears. The present invention successfully prepares a ferroelectric material with a perovskite structure by partially non-equivalently substituting bismuth element for the A position of the perovskite-type barium strontium titanate ferroelectric film.

[0084] Figure 2 The hysteresis loops of the low hysteresis and high dielectric tunable ferroelectric material prepared in Example 1 at voltages of 10V, 20V and 30V, respectively. Figure 2 It can be seen that the hysteresis loop of the ferroelectric material is relatively slender and the hysteresis is small.

[0085] Figure 3 The dielectric constant of the low hysteresis high dielectric tunable ferroelectric material prepared in Example 1 varies with temperature (25-300°C) at 1kHz, 10kHz and 100kHz respectively. Figure 3 It can be seen that the dielectric constant of the ferroelectric material at different frequencies decreases with increasing temperature, and the dielectric constant in the temperature range of 25 to 300 ° C can be maintained between 220 and 310; Figure 4 As shown in the figure, the dielectric constant (ε′) at 150°C 150℃) as the benchmark, Δε' represents the difference between the dielectric constant at any temperature and the dielectric constant at 150℃, and the calculated dielectric constant change rate (Δε' / ε' 150 ℃) is less than ±15% in the temperature range of 25 to 300 ℃ and the frequency range of 1 to 100 kHz, indicating that the dielectric constant of the ferroelectric material prepared by the present invention has excellent temperature stability and frequency stability.

[0086] Figure 5 The dielectric loss curves of the low hysteresis high dielectric tunable ferroelectric material prepared in Example 1 at frequencies of 1kHz, 10kHz and 100kHz are plotted against temperature (25-300°C). Figure 5 It can be seen that the dielectric loss of the ferroelectric material in the test temperature range is always lower than 0.15, especially the dielectric loss at 100kHz does not exceed 0.03 in the temperature range of 25-300℃.

[0087] Figure 6 The dielectric constant variation curves of the low hysteresis high dielectric tunable ferroelectric material prepared in Example 1 at room temperature at 1 kHz, 10 kHz and 100 kHz respectively are as follows: Figure 6 It can be seen that the dielectric constant of the ferroelectric material decreases with the increase of bias voltage in the test temperature range, and Figure 6 There is no obvious hysteresis in the dielectric constant as the voltage rises and falls.

[0088] Figure 7 The dielectric tuning rate of the low hysteresis and high dielectric tunable ferroelectric material prepared in Example 1 at different frequencies, wherein: Figure 7 (a) is 1kHz, Figure 7 (b) is 10kHz, Figure 7 (c) is 100kHz; Figure 7 It can be seen that the dielectric tuning rate of the ferroelectric material at room temperature, 1kHz and 12V voltage reaches 21.88%; the dielectric tuning rate at room temperature, 10kHz and 12V voltage reaches 21.62%; the dielectric tuning rate at room temperature, 100kHz and 12V voltage reaches 21.43%; this shows that the low hysteresis and high dielectric tunable ferroelectric material prepared by the present invention has basically no change in the dielectric tuning rate within 1-100kHz, and the hysteresis phenomenon is small, and can be widely used in ferroelectric phase shifters, ferroelectric tunable filters and variable capacitors, etc.

Claims

1. A low hysteresis high dielectric tunable ferroelectric material, characterized in that: The chemical formula of the ferroelectric material is (Sr 0.6 Ba 0.4 ) (1-1.5x) Bi x TiO3, where 0<x<0.

4.

2. The low hysteresis high dielectric tunable ferroelectric material according to claim 1, characterized in that: Preferably, the value of x is: 0.05≤x≤0.

3.

3. The low hysteresis high dielectric tunable ferroelectric material according to claim 1, characterized in that: The ferroelectric material is a thin film material with a thickness of 200-400 nm.

4. The low hysteresis high dielectric tunable ferroelectric material according to claim 1, characterized in that: The ferroelectric material is a perovskite structure and has defect dipole characteristics.

5. A method for preparing the low hysteresis high dielectric tunable ferroelectric material according to any one of claims 1 to 4, characterized in that: The steps include: Step 1: According to the chemical formula (Sr 0.6 Ba 0.4 ) (1-1.5x) Bi x Barium acetate, strontium acetate and bismuth nitrate are weighed in the stoichiometric ratio of each element in TiO3 to obtain a mixed raw material; the mixed raw material is dissolved in a mixed solution of ethylene glycol methyl ether, acetic acid and ammonia water, and heated and stirred at 40 to 60° C. for 4 to 6 hours to obtain a solution A; Step 2: According to the chemical formula (Sr 0.6 Ba 0.4 ) (1-1.5x) Bi x The stoichiometric ratio of the Ti element in TiO3 was 4-6 hours after the tetrabutyl titanate solution was weighed and mixed with the acetylacetone solution to obtain solution B. Step 3: Mix solution A and solution B, stir, and age for 20 to 35 hours to obtain (Sr) with a molar concentration of 0.2 to 0.3 mol / L. 0.6 Ba 0.4 ) (1-1.5x) Bi x TiO3 precursor solution; Step 4: Spin-coat the precursor solution obtained in step 3 onto the pretreated substrate, then perform annealing and crystallization in a rapid annealing furnace, and repeat the spin-coating and annealing operation until a film with a thickness of 200 to 400 nm is obtained, i.e., a low hysteresis and high dielectric tunable ferroelectric material.

6. The method for preparing the low hysteresis high dielectric tunable ferroelectric material according to claim 5, characterized in that: In the step 1, the volume ratio of ethylene glycol methyl ether: acetic acid: ammonia water is (5-6): (5-6): (0.5-1).

7. The method for preparing the low hysteresis high dielectric tunable ferroelectric material according to claim 5, characterized in that: In the step 2, the volume ratio of tetrabutyl titanate solution to acetylacetone solution is (4-5):

1.

8. The method for preparing the low hysteresis high dielectric tunable ferroelectric material according to claim 5, characterized in that: The specific process of spin coating annealing in step 4 is as follows: 1) dropping the precursor solution onto the substrate for spin coating, first rotating at a speed of 500 to 800 rpm for 5 to 10 seconds, and then rotating at a speed of 3000 to 4000 rpm for 25 to 35 seconds to obtain a spin-coated film; 2) placing the spin-coated film obtained in step 1) in a rapid annealing furnace and annealing at 300-350° C. for 3-5 min, and then annealing at 560-650° C. for 5-10 min; 3) Repeat step 1) and step 2) until a film with a thickness of 200-400 nm is obtained, that is, a low hysteresis and high dielectric tunable ferroelectric material.

9. The method for preparing the low hysteresis high dielectric tunable ferroelectric material according to claim 5, characterized in that: The pretreatment process of the substrate in step 4 is: the substrate is cleaned in an ultrasonic cleaning machine using acetone, ethanol and distilled water in sequence for 5-15 minutes, and after cleaning, the substrate is blown dry using high-purity nitrogen.

10. Use of the low hysteresis and high dielectric tunable ferroelectric material according to any one of claims 1 to 4 or the low hysteresis and high dielectric tunable ferroelectric material prepared by the preparation method according to any one of claims 5 to 9 in a ferroelectric phase shifter or a dielectric tunable capacitor.