Optical fiber surface high-temperature-resistant coating process

Through the multi-layer coating process and the use of modified polyimide coatings, the problem of optical fibers being easily broken in high-temperature environments is solved, and the high-temperature, aging and radiation resistance of optical fibers are achieved, ensuring stability in harsh environments use.

CN118993576APending Publication Date: 2024-11-22WEIHAI WEIXIN OPTICAL FIBER TECH CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410834788.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing optical fibers are prone to fatigue and microcracks in high temperature environments, resulting in natural fractures and cannot meet the reliability requirements in high temperature environments.

Method used

Using a multi-layer coating process, including drying with high purity gases, drawing to form bare fibers with uniform diameters, pre-coating and curing, using modified polyimide coatings to combine with ordinary coatings, and ensuring thickness and Concentricity, achieve high temperature resistance.

Benefits of technology

It improves the high temperature, aging and radiation resistance of the optical fiber, making it stable for long-term use in harsh high temperature environments and prevents signal distortion.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a high-temperature-resistant coating process for the surface of an optical fiber. The high-temperature-resistant coating process comprises the following steps: step 1, cleaning an optical fiber preform with pure water, and drying the preform with high-purity gas; step 2, performing wire drawing on the optical fiber preform on wire drawing equipment to obtain a bare optical fiber with a uniform diameter; step 3, pre-coating is carried out, and the bare fiber passes through a pre-coating device under traction; step 4, performing pre-curing on the pre-coated bare optical fiber; step 5, repeating the steps 3-4 to coat and cure the bare optical fiber; and 6, after the diameter is detected by the diameter detection device, the wire is stored on a take-up reel of the take-up device. Compared with the prior art, the high-temperature-resistant coating process for the surface of the optical fiber has the advantages that the high-temperature-resistant use can be realized, the use function of the optical fiber is ensured, and the durability is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of high temperature resistant optical fiber, and in particular to a high temperature resistant coating process for the surface of an optical fiber. Background Art

[0002] With the development of optical fiber technology, the application scope of optical fiber is becoming wider and wider. The application of optical fiber has been extended to the fields of laser energy transmission, sensing technology, etc., and the application scope has also been extended to various high-temperature and harsh environments. This has gradually increased the requirements for the mechanical and high-temperature resistance properties of optical fiber.

[0003] As an information transmission material, the core and cladding of optical fiber are mainly composed of quartz. The cladding is covered with a coating layer to protect the optical fiber. Ordinary optical fiber uses UV-curing acrylic resin as a coating. Its operating temperature is -60℃-85℃. When the temperature is higher than 85℃, the fatigue process of the optical fiber may be accelerated, causing micro cracks on the surface of the optical fiber to expand, which may easily cause the optical fiber to break naturally and cannot meet the reliability requirements of optical fiber transmission in high temperature environments. Summary of the invention

[0004] The technical problem to be solved by the present invention is to overcome the above technical defects and provide a high-temperature resistant coating process for the surface of an optical fiber that can withstand high temperatures, ensure the optical fiber's use function, and has high durability.

[0005] In order to solve the above technical problems, the technical solution provided by the present invention is: a high-temperature resistant coating process for optical fiber surface, comprising the following steps: Step 1: After cleaning the optical fiber preform with pure water, the preform is dried with high-purity gas; Step 2: Drawing the optical fiber preform on a drawing device to obtain a bare optical fiber with uniform diameter; Step 3: Pre-coating, the bare optical fiber passes through the pre-coating device under traction; Step 4: Pre-curing the pre-coated bare optical fiber; Step 5: Repeat steps 3-4 to coat and cure the bare optical fiber; Step 6: After detection by a diameter detection device, it is stored on the take-up reel of the take-up device.

[0006] Preferably, during the specific operation in step 2, the front end of the optical fiber preform is melted in a high-temperature graphite furnace and forms a cone under the traction of gravity and a traction device, and is passed through a bare optical fiber diameter detection instrument to be drawn at a constant speed to obtain a bare optical fiber with uniform diameter.

[0007] Preferably, step 5 includes sizing the optical fiber after each coating, wherein the first coating thickness is less than 10 μm, the second coating thickness is less than 20 μm, and the third coating thickness is less than 30 μm, and the target thickness is reached after three coatings.

[0008] Preferably, the pre-curing in step 4 is performed by ultraviolet light curing.

[0009] Preferably, the repeated coating in step 5 is a modified polyimide coating.

[0010] Preferably, in step 2, a high temperature furnace is used for wire drawing at a temperature of 1800-2000° C., and the wire drawing is annealed and forcedly cooled after exiting the furnace.

[0011] Preferably, the first coating is a common coating.

[0012] Preferably, the density of the polyimide coating is 1.38-1.43 g / cm 3 .

[0013] The advantages of the present invention over the prior art are as follows: in the present invention, a new structural design is performed on the surface coating of the optical fiber, a polyimide coating is compounded with an ordinary coating, and the polyimide coating set by multi-layer coating and curing makes the optical fiber have high temperature resistance and prevents signal distortion. Compared with conventional coated optical fibers, the optical fiber has the characteristics of high temperature resistance, aging resistance, radiation resistance, stability and durability, so that the optical fiber can be used for a long time in a high temperature and harsh environment. At the same time, the present invention also provides an additional diameter detection instrument, which ensures the diameter deviation and concentricity through sizing treatment after each coating. DETAILED DESCRIPTION

[0014] The present invention is described in further detail below.

[0015] References to embodiments of the present invention will now be provided in detail, one or more examples of which are described below. Each example is provided as an explanation rather than a limitation of the present invention. In fact, it will be apparent to those skilled in the art that various modifications and variations may be made to the present invention without departing from the scope or spirit of the present invention. For example, a feature illustrated or described as part of one embodiment may be used in another embodiment to produce a further embodiment.

[0016] Therefore, it is intended that the present invention covers such modifications and variations that fall within the scope of the appended claims and their equivalents. Other objects, features and aspects of the present invention are disclosed in or are obvious from the following detailed description. Those of ordinary skill in the art will appreciate that this discussion is only a description of exemplary embodiments and is not intended to limit the broader aspects of the present invention.

[0017] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0018] A high temperature resistant coating process for optical fiber surface, characterized in that it comprises the following steps: Step 1: After cleaning the optical fiber preform with pure water, the preform is dried with high purity gas; Step 2: Drawing the optical fiber preform on a drawing device to obtain a bare optical fiber with uniform diameter; Step 3: Pre-coating, the bare optical fiber passes through the pre-coating device under traction; Step 4: Pre-curing the pre-coated bare optical fiber; Step 5: Repeating steps 3-4 to coat and cure the bare optical fiber; Step 6: After detection by a diameter detection device, the bare optical fiber is stored on a take-up reel of a take-up device.

[0019] When the present invention is implemented,

[0020] After the optical fiber preform is cleaned with pure water, it is dried with high-pressure and high-purity gas. The front end of the optical fiber preform is melted in a high-temperature graphite furnace and forms a cone under the traction of gravity and traction equipment. It passes through a bare optical fiber diameter detection instrument and is drawn at a constant speed to obtain a bare optical fiber with uniform diameter. The temperature is 1800-2000°C. After being drawn out of the furnace, it is annealed and forced to cool. The forced cooling includes natural cooling for 3-6m. The speed of the traction device is set to 3m / min.

[0021] A pre-coating is performed, and the bare optical fiber passes through the pre-coating device under traction. The first coating is a common coating, and the diameter is set to a coating thickness of less than 10μm. After UV curing, a second coating is performed, and the second coating is a modified polyimide coating. The diameter is set to a second coating thickness of less than 20μm. After UV curing, a third coating is performed, and the diameter is set to a third coating thickness of less than 30μm. UV curing is performed, and the diameter detection device is detected and then stored on the take-up reel of the take-up device. The density of the polyimide coating is 1.38-1.43g / cm 3 .

[0022] The contents not described in detail in this specification belong to the prior art known to professional and technical personnel in this field.

[0023] The present invention and its implementation methods are described above, but such description is not restrictive, and what is shown is only one of the implementation methods of the present invention, and the actual structure is not limited thereto. In short, if ordinary technicians in the field are inspired by it, without departing from the purpose of the invention, they can design a structure and embodiment similar to the technical solution without creativity, which should belong to the protection scope of the present invention.

Claims

1. A high temperature resistant coating process for optical fiber surface, characterized in that: The following steps are involved: Step 1: Clean the optical fiber preform with pure water and then dry the preform with high-purity gas; Step 2: Drawing the optical fiber preform on a drawing device to obtain a bare optical fiber with uniform diameter; Step 3: Pre-coating is performed, and the bare optical fiber passes through the pre-coating device under traction; Step 4: Pre-curing the pre-coated bare optical fiber; Step 5: Repeat steps 3-4 to coat and cure the bare optical fiber; Step 6: After the diameter detection device detects, the wire is stored on the wire take-up reel of the wire take-up device.

2. A high temperature resistant coating process for optical fiber surface according to claim 1, characterized in that: In the specific operation of step 2, the front end of the optical fiber preform is melted in a high-temperature graphite furnace and formed into a cone under the traction of gravity and traction equipment, and is passed through a bare optical fiber diameter detection instrument to be drawn at a constant speed to obtain a bare optical fiber with uniform diameter.

3. A high temperature resistant coating process for optical fiber surface according to claim 1, characterized in that: The step 5 includes sizing the optical fiber after each coating, wherein the first coating thickness is less than 10 μm, the second coating thickness is less than 20 μm, and the third coating thickness is less than 30 μm, and the target thickness is reached after three coatings.

4. The high temperature resistant coating process for optical fiber surface according to claim 1, characterized in that: The pre-curing in step 4 is performed by ultraviolet light curing.

5. The high temperature resistant coating process for optical fiber surface according to claim 3, characterized in that: The repeated coating in step 5 is a modified polyimide coating.

6. A high temperature resistant coating process for optical fiber surface according to claim 2, characterized in that: In step 2, a high temperature furnace is used for wire drawing at a temperature of 1800-2000° C., and the wire drawing is annealed and forcedly cooled after being taken out of the furnace.

7. The optical fiber surface high temperature resistant coating process according to claim 3, characterized in that: The first coating is a common coating.

8. The high temperature resistant coating process for optical fiber surface according to claim 5, characterized in that: The density of the polyimide coating is 1.38-1.43 g / cm 3 .

Citation Information

Patent Citations

  • High temperature resistant fiber and processing technology thereof

    CN102360096A

  • High-temperature-resistance optical fiber

    CN103777269A

  • Irradiation-resistant optical fiber and preparation method thereof

    CN110133796A

  • Method for manufacturing polyimide coated fiber

    JP2008081335A