Fly ash doped cement clinker as well as preparation method and application thereof
By calcining limestone, converter slag, sandstone and fly ash with coal powder and fly ash, the heavy metal morphology is adjusted, and the problem of high leaching of heavy metals in existing cement clinker is solved, and good mechanical properties that meet building material standards are achieved and low heavy metal leaching amount.
Patent Information
- Application Number
- CN202411114043.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-22
AI Technical Summary
Cement clinker produced by existing cement kiln collaborative treatment of fly ash technology has poor stability effect on heavy metals, resulting in high leaching of heavy metals and cannot meet the standard requirements of building materials.
Mix limestone, converter slag, sandstone and fly ash and grind it, add coal powder and fly ash for calcination, adjust the amount and particle size of fly ash, change the morphological distribution of heavy metals through calcination, and transform it into cement clinker. In a form that is not easy to leaching, the amount of heavy metal leaching is reduced.
The prepared fly ash doped cement clinker has good mechanical properties and a low leaching amount of heavy metals, meeting the requirements of building materials. The flexural strength is 7.13MPa in 28 days, the compressive strength is 46.98MPa, and the heavy metal leaching amount is low. In national standards.
Smart Images

Figure CN118993584A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of solid waste treatment, and in particular to fly ash-doped cement clinker and a preparation method and application thereof. Background Art
[0002] With the rapid development of China's economy in recent years, the living standards of our residents have been greatly improved, and the process of urbanization is also very rapid. However, with the rapid development of urbanization and the improvement of people's living standards, a large amount of domestic waste has also been brought accordingly.
[0003] Incineration is a common method of treating domestic waste in countries around the world. However, the incineration process of domestic waste will produce secondary pollution, and its incineration products contain substances that are harmful to the human body and the environment, such as: particulate pollutants, acidic gases, volatile heavy metals, dioxins, and furans, etc., which are especially produced in large quantities when the waste is not incinerated sufficiently, and are highly toxic. After the particulate pollutants in the incineration process are captured by the dust collector, they will remain in the form of fly ash, while volatile heavy metals and dioxins are mostly adsorbed on the fly ash, which is why fly ash can cause serious pollution, and for this reason, fly ash is listed as hazardous waste. After the waste is incinerated, the amount of fly ash produced is about 10% of the original volume of the waste, and the mass is about 3% to 5% of the original mass of the waste. How to properly deal with fly ash is a major problem at present, and it also hinders the application of incineration technology to treat waste.
[0004] At present, fly ash can be used as raw material for cement production through fly ash co-processing in cement kilns, realizing the reuse of fly ash. However, the cement clinker produced by the existing fly ash co-processing technology in cement kilns has poor stabilization effect on heavy metals, resulting in high leaching of heavy metals in the solidified material, which cannot meet the standard requirements of building materials. Summary of the invention
[0005] The purpose of the present invention is to provide a fly ash-doped cement clinker and a preparation method and application thereof. The fly ash-doped cement clinker obtained by the preparation method provided by the present invention has a good stabilizing effect on heavy metals, and the prepared mortar has a low heavy metal leaching amount, which can meet the standard requirements of building materials.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] A method for preparing fly ash-doped cement clinker comprises the following steps:
[0008] (1) limestone, converter slag, sandstone and fly ash are mixed and ground to obtain cement raw material;
[0009] (2) mixing the cement raw meal obtained in step (1) with coal powder and fly ash and calcining the mixture to obtain fly ash-doped cement clinker;
[0010] The mass of the fly ash in step (2) is 2-3% of the mass of the cement raw material.
[0011] Preferably, the mass of the fly ash in step (2) is 2.5-3% of the mass of the cement raw material.
[0012] Preferably, in step (1), the mass ratio of limestone, converter slag, sandstone and fly ash is (90-93): (2-3): (2-5): (2-3).
[0013] Preferably, in step (1), the mass ratio of limestone, converter slag, sandstone and fly ash is (91-92): (2-2.5): (3-4): (2-2.5).
[0014] Preferably, the mass of the coal powder in step (2) is 7-9% of the mass of the cement raw material.
[0015] Preferably, the particle size of the fly ash in step (2) is 12 to 18 μm.
[0016] Preferably, the particle size of the coal powder in step (2) is 16 to 22 μm.
[0017] Preferably, the calcination temperature in step (2) is 1400-1480° C., and the calcination time is 30-40 min.
[0018] The present invention also provides fly ash-doped cement clinker prepared by the preparation method described in the above technical solution.
[0019] The present invention also provides the use of the fly ash-doped cement clinker described in the above technical solution in cement mortar.
[0020] The present invention provides a method for preparing fly ash-doped cement clinker, comprising the following steps: (1) mixing limestone, converter slag, sandstone and fly ash and grinding them to obtain cement raw material; (2) mixing the cement raw material obtained in step (1) with coal powder and fly ash and calcining them to obtain fly ash-doped cement clinker; the mass of the fly ash in step (2) is 2-3% of the mass of the cement raw material. The present invention mixes fly ash with cement raw material, and changes the form distribution of heavy metals in fly ash and cement raw material by calcining, so that the heavy metals in fly ash and cement raw material are converted into a form that is not easy to be leached (residue state) in cement clinker, and by adjusting the addition amount of fly ash, more heavy metals in cement clinker exist in a form that is not easy to be leached (residue state), so that the mortar has a lower heavy metal leaching amount without affecting the mechanical properties, thereby meeting the use requirements of building materials. Experimental results show that the mortar prepared from the fly ash-doped cement clinker obtained by the preparation method provided by the present invention has a flexural strength of 7.13 MPa and a compressive strength of 46.98 MPa after 28 days of curing; the heavy metal ions in the mortar are leached out by the national standard 30810 method, and the As leaching amount is 12.63 μg / L, the Cd leaching amount is 14.92 μg / L, the Cr leaching amount is 52.82 μg / L, the Cu leaching amount is 84.34 μg / L, the Mn leaching amount is 346.42 μg / L, the Ni leaching amount is 89.91 μg / L, the Pb leaching amount is 18.32 μg / L, and the Zn leaching amount is 534.33 μg / L, which has good mechanical properties and low heavy metal leaching amount. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 is a bar graph showing the percentage distribution of heavy metals in different chemical forms in the fly ash in Example 1 of the present invention;
[0022] Figure 2 This is a bar graph showing the percentage of heavy metals in different chemical forms in the fly ash-doped cement clinker prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0023] The present invention provides a method for preparing fly ash-doped cement clinker, comprising the following steps:
[0024] (1) limestone, converter slag, sandstone and fly ash are mixed and ground to obtain cement raw material;
[0025] (2) mixing the cement raw meal obtained in step (1) with coal powder and fly ash and calcining the mixture to obtain fly ash-doped cement clinker;
[0026] The mass of the fly ash in step (2) is 2-3% of the mass of the cement raw material.
[0027] The invention mixes limestone, converter slag, sandstone and fly ash and grinds them to obtain cement raw material.
[0028] In the present invention, the limestone and sandstone are preferably derived from natural mining; the converter slag is preferably derived from steel plant waste; and the fly ash is preferably derived from coal yard waste.
[0029] In a specific embodiment of the present invention, the chemical compositions of the limestone, converter slag, sandstone and fly ash are shown in Table 1.
[0030] Table 1 Chemical composition of limestone, converter slag, sandstone and fly ash Unit: (%)
[0031]
[0032]
[0033] In a specific embodiment of the present invention, the heavy metal contents of the limestone, converter slag, sandstone and fly ash are as shown in Table 2.
[0034] Table 2 Heavy metal content of limestone, converter slag, sandstone and fly ash Unit: (mg / kg)
[0035] raw material As Cd Cr Cu Mn Ni Pb Zn limestone 1.91 0.07 15.06 9.59 131.46 37.77 9.80 5.38 sandstone 3.02 0.05 114.73 19.68 254.38 20.40 4.11 17.04 Fly ash 7.24 0.31 17.07 18.17 188.19 11.40 17.45 26.09 Converter slag 10.99 0.13 104.98 19.81 2744.86 18.15 3.58 39.66
[0036] In the present invention, the mass ratio of the limestone, converter slag, sandstone and fly ash is preferably (90-93): (2-3): (2-5): (2-3), more preferably (91-92): (2-2.5): (3-4): (2-2.5), and further preferably 91: 2: 3: 2. The present invention limits the mass ratio of limestone, converter slag, sandstone and fly ash to the above range to ensure that the prepared cement clinker has good mechanical properties and meets national standards. At the same time, during the calcination of cement, the above raw materials can make more heavy metals in the raw materials into a form that is not easy to leach through the coordination of the raw material content, thereby reducing the amount of heavy metal leaching from the cement clinker.
[0037] The present invention has no special limitation on the mixing method and operation of the limestone, converter slag, sandstone and fly ash, and the mixing method and operation commonly used by those skilled in the art can be adopted.
[0038] The present invention has no special limitation on the grinding method and operation, and the grinding method and operation commonly used by those skilled in the art can be adopted.
[0039] In the present invention, the particle size of the cement raw material is preferably 20-28 μm, more preferably 25 μm. In the present invention, limiting the particle size of the cement raw material to the above range can facilitate the calcination of cement.
[0040] After obtaining the cement raw meal, the present invention mixes the cement raw meal with coal powder and fly ash and then calcines the mixture to obtain fly ash-doped cement clinker.
[0041] In a specific embodiment of the present invention, the chemical composition of the coal powder and fly ash is shown in Table 3.
[0042] Table 3 Chemical composition of coal powder and fly ash Unit: (%)
[0043]
[0044]
[0045] In a specific embodiment of the present invention, the heavy metal contents of the coal powder and fly ash are as shown in Table 4.
[0046] Table 4 Heavy metal content of coal powder and fly ash Unit: (mg / kg)
[0047] raw material As Cd Cr Cu Mn Ni Pb Zn Coal powder 2.36 0.15 9.90 8.80 89.31 10.78 11.17 17.73 Fly ash 37.59 47.83 96.71 264.89 647.61 64.07 722.46 4294.18
[0048] In the present invention, the mass of the coal powder is preferably 7-9% of the mass of the cement raw material, and more preferably 8%. The present invention limits the amount of coal powder added to the above range to ensure that sufficient energy is provided for the calcination of cement, promote the sintering of cement clinker, ensure the mechanical properties of cement clinker, and ensure that the heavy metals in the fly ash are further converted into a form that is not easy to leach in the cement clinker.
[0049] In the present invention, the particle size of the coal powder is preferably 16-22 μm, more preferably 18-20 μm. The present invention limits the particle size of the coal powder to the above range to ensure the full combustion of the coal powder and better provide heat for the calcination of cement.
[0050] In the present invention, when the particle size of the coal powder is not within the above range, the present invention preferably pre-treats the coal powder before use; the pre-treatment preferably includes cleaning and grinding. The present invention does not specifically limit the operations of the cleaning and grinding, and the cleaning and grinding commonly used by those skilled in the art may be adopted. In the present invention, the mass of the fly ash is 2-3%, preferably 2.5-3%, of the mass of the cement raw material. In the present invention, the particle size of the fly ash is preferably 12-18 μm, more preferably 14-16 μm. The present invention limits the addition amount and particle size of the fly ash to the above range to ensure that the cement clinker has a low heavy metal leaching amount while having good mechanical properties.
[0051] In the present invention, the calcination temperature is preferably 1400-1480°C, more preferably 1420-1460°C; the calcination time is preferably 30-40 minutes, more preferably 35 minutes. The present invention limits the calcination temperature and time to the above ranges to ensure that the cement clinker has good mechanical properties, and at the same time ensures that more heavy metals in the fly ash can be converted into a form that is not easy to leach (residue state) during the calcination process, thereby improving the stability of heavy metals in the cement clinker, thereby ensuring that the mortar prepared from the cement clinker has a lower heavy metal leaching amount.
[0052] The present invention mixes fly ash with cement raw meal, changes the form distribution of heavy metals in the fly ash and cement raw meal by calcination, and converts the heavy metals in the fly ash and cement raw meal into a form (residue state) that is not easily leached in cement clinker. By adjusting the added amount of fly ash, more heavy metals in the cement clinker exist in a form (residue state) that is not easily leached, and the mortar has a lower heavy metal leaching amount without affecting the mechanical properties of the mortar, thereby meeting the use requirements of building materials.
[0053] The present invention also provides fly ash-doped cement clinker prepared by the preparation method described in the above technical solution.
[0054] In a specific embodiment of the present invention, the chemical composition of the cement clinker is as shown in Table 5.
[0055] Table 5 Chemical composition of cement clinker Unit: (%)
[0056] CaO <![CDATA[SiO2]]> MgO <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> <![CDATA[K2O]]> <![CDATA[TiO2]]> SrO Cl MnO <![CDATA[SO3]]> Cement clinker 54.07 18.013 2.972 3.539 3.771 0.675 0.061 0.031 0.076 1.23 <![CDATA[P2O5]]> PbO <![CDATA[Na2O]]> ZnO CuO <![CDATA[ZrO2]]> <![CDATA[CeO2]]> BaO <![CDATA[Cr2O3]]> <![CDATA[Rb2O]]> Cement clinker 0.128 0.01 0.638 0.039 0.015 0.03
[0057] In a specific embodiment of the present invention, the heavy metal content of the cement clinker is as shown in Table 6.
[0058] Table 6 Heavy metal content of cement clinker Unit: (mg / kg)
[0059] As Cd Cr Cu Mn Ni Pb Zn Cement clinker 13.03 1.21 26.07 17.38 325.98 63.80 34.24 155.97
[0060] The present invention also provides the use of the fly ash-doped cement clinker described in the above technical solution in cement mortar.
[0061] In the present invention, the cement mortar is preferably obtained by mixing fly ash-doped cement clinker, standard sand, water and gypsum, followed by curing and oxidation treatment.
[0062] In the present invention, the mass ratio of the fly ash-doped cement clinker to the standard sand is preferably (0.8-1.2):(2.4-3.6).
[0063] The present invention has no special requirements on the amount of water and gypsum used and the operation of mixing and curing, and the technical solutions well known in the art can be adopted.
[0064] The cement mortar prepared from the fly ash-doped cement clinker provided by the invention has a low heavy metal leaching rate.
[0065] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0066] Example 1
[0067] A method for preparing fly ash-doped cement clinker comprises the following steps:
[0068] (1) limestone, converter slag, sandstone and fly ash are mixed and ground to obtain cement raw material; the mass ratio of the limestone, converter slag, sandstone and fly ash is 91:2:3:2; the chemical compositions of the limestone, converter slag, sandstone and fly ash are shown in Table 1; the heavy metal contents of the limestone, converter slag, sandstone and fly ash are shown in Table 2;
[0069] (2) The cement raw material obtained in step (1), the coal powder with a particle size of 16 to 22 μm after washing and grinding, and the fly ash with a particle size of 12 to 18 μm are mixed and calcined at 1450° C. for 35 min to obtain fly ash-doped cement clinker; the mass of the fly ash is 3% of the mass of the cement raw material; the mass of the coal powder is 8% of the mass of the cement raw material; the chemical composition of the coal powder and the fly ash is shown in Table 3; the heavy metal content of the coal powder and the fly ash is shown in Table 4.
[0070] The chemical composition of the fly ash-doped cement clinker prepared by the preparation method is shown in Table 5; the heavy metal content of the fly ash-doped cement clinker is shown in Table 6.
[0071] Application Example 1
[0072] The fly ash-doped cement clinker prepared in Example 1, standard sand, water and gypsum were mixed in a mass ratio of 1:3:0.5:0.05, and after being molded and solidified, they were placed in a curing room for curing. After 24 hours, the mixture was demolded and placed in water at a temperature of 20°C for further curing to obtain cement mortar.
[0073] Test Case
[0074] (I) The heavy metal content of the fly ash-doped cement clinker obtained in Example 1 was determined by microwave full-amount digestion method. The specific determination steps are as follows: first, 0.100 g of fly ash-doped cement clinker was weighed and placed in a polytetrafluoroethylene digestion tank. Then, 6 mL of HNO3, 2 mL of HCl, and 1 mL of HF, then cover the lid of the digestion tank. It is important to ensure that the lid of the digestion tank is balanced with the plug inside. The identification method is that the top of the lid is flat and there is no bump. Then put the digestion tank into a microwave digestion instrument, heat it to 200°C at a power of 1500kW and keep it warm for a period of time to allow the sample to be completely digested. After the digestion is completed, use ultrapure water to make the volume of the digested solution to 50mL, and finally use ICP-MS to determine the content of heavy metals in the test solution. The target heavy metals detected are arsenic (As), cadmium (Cd), chromium (Cr), copper (Cu), manganese (Mn), nickel (Ni), lead (Pb) and zinc (Zn) The total content;
[0075] The digestion program settings of the microwave digestion instrument are shown in Table 7.
[0076] Table 7 Digestion program of microwave digestion instrument
[0077]
[0078]
[0079] (ii) using the BCR continuous leaching method to determine the chemical forms of heavy metals in the fly ash in Example 1 and the obtained fly ash-doped cement clinker;
[0080] During the leaching process, leaching is carried out in the order of acid exchangeable state, iron and manganese oxidation state, organic state and residual state;
[0081] The extractant settings for the BCR continuous extraction method are shown in Table 8;
[0082] Table 8 Extractants for BCR continuous extraction method
[0083] Chemical form Extraction agent Acid exchangeable state 0.11M glacial acetic acid Iron and manganese oxidation state 0.5M Hydroxylamine Hydrochloride Organic 30% hydrogen peroxide + 1M ammonium acetate Residue Mixed acid (nitric acid + hydrochloric acid + hydrofluoric acid)
[0084] The specific operation steps of BCR continuous extraction method are as follows:
[0085] The first step is to determine the acid exchangeable state. First, use a balance to weigh 1.00g of fly ash or fly ash-doped cement clinker into a 50mL centrifuge tube, then add 40mL of the prepared 0.11mol / L glacial acetic acid, and use a gyroscopic oscillator to oscillate and extract for 16 hours at room temperature. During the oscillation process, the sample in the centrifuge tube should be kept in a suspended state, and the oscillation frequency is about 250r / min. After the oscillation, use a centrifuge (3000r / min, 20min) for centrifugal separation, extract 20mL of the upper clear liquid into a sample bottle, and store it in a refrigerator at 4°C for testing. The remaining upper liquid is discarded, and then 20mL of pure water is added to the centrifuge tube to wash the residue. After oscillation for 15min, centrifuge (3000r / min, 20min) is performed again, and the washing liquid is poured out;
[0086] The second step is to determine the oxidation state of iron and manganese. 40 mL of 0.5 mol / L NH2OH·HCl is added to the residue of the previous step, and the mixture is shaken and extracted for 16 h. The mixture is centrifuged (3000 r / min, 20 min) and the remaining steps are the same as the first step. The supernatant obtained by centrifugation and washing is stored in a refrigerator, and the solid residue is used in the next step.
[0087] The third step is to determine the organic state. Add 10mL of H2O2 to the residue of the second step, and digest it under oscillation at room temperature for 1h. Then digest it at 85℃ in a water bath for 1h. Then heat it until the liquid volume in the centrifuge tube is reduced to less than 3mL. Then add 10mL of H2O2 to the centrifuge tube, and continue heating in a water bath until the liquid volume is reduced to about 1mL. Be careful not to evaporate the liquid. After cooling, add 50mL of 1mol / L NH4OAc solution to the residue, and extract it under oscillation at room temperature for 16h. The remaining steps are the same as the first step. The supernatant obtained by centrifugation and washing is stored in the refrigerator, and the solid residue is left for the next step.
[0088] The fourth step is to determine the residue state. Add 20 mL of pure water to the solid residue from the previous step, oscillate with an oscillator for 15 minutes, separate using a centrifuge (3000 r / min, 20 minutes), pour off the supernatant, leaving the solid residue, evaporate the solid residue in a water bath, collect the residue thoroughly, and then use microwave full-volume digestion to digest it. The digestion method is the same as the above-mentioned microwave full-volume digestion method to obtain a digested solution to be tested. Finally, the obtained test solution is used to detect the content of heavy metals using ICP-MS.
[0089] (III) The strength of the cement mortar in Example 1 is measured using a flexural and compressive testing machine. The loading rate for testing the flexural strength is 0.05 kN / s, and the loading rate for testing the compressive strength is 2.4 kN / s.
[0090] (IV) The national standard 30810 method (GB / T 30810-2014 Determination of leached heavy metals in cement mortar) is used to test the heavy metal leaching amount of the cement mortar in Example 1. The specific test steps are as follows:
[0091] Cement mortar was dried in an oven at 105°C, ground with a ball mill, and particles of 0.125 mm to 0.25 mm were collected as the sample to be tested; at room temperature, 10.00 g of the sample was weighed into a 1 L beaker, 500 mL of ultrapure water was added, and the sample was placed on a magnetic stirrer and stirred, and the sample was kept in a suspended state during the stirring process; during the stirring process, the pH value in the beaker was measured with a pH meter, and a pH adjusting solution was added with a dropper (100 mL of sulfuric acid was slowly added to 200 mL of water, and 50 mL of nitric acid was added to 100 mL of water, and the two solutions were cooled to room temperature and then mixed), so that the pH value of the liquid in the beaker was maintained at 7.0 ± 0.5 and stirred for 2 hours; after the stirring was completed, After standing for 5 minutes, filter and collect the filtrate using a Buchner funnel, wash the residue 3 times with water, merge the filtrate into the leachate, and make up the volume of the leachate in a 1L volumetric flask; then collect the residue and transfer it to a beaker, add 500mL of water again, place it on a magnetic stirrer for stirring and add a pH adjusting solution to adjust the pH value of the liquid in the beaker to 3.2, and keep the pH of the liquid at 3.2±0.5 and stir for 7 hours. After standing for 5 minutes, filter and collect the filtrate using a Buchner funnel, wash the residue 3 times with water, merge the filtrate into the leachate, and make up the volume in a 1L volumetric flask; finally, mix the liquids in the two 1L volumetric flasks and make up the volume in a 2L volumetric flask, and use ICP-MS to determine the content of heavy metals.
[0092] The heavy metal contents in the fly ash in Example 1 and the prepared fly ash-doped cement clinker and the heavy metal limits for cement clinker in "GB / T30760-2014 Technical Specifications for Co-treatment of Solid Wastes in Cement Kilns" are shown in Table 9.
[0093] Table 9 Heavy metal content in fly ash-doped cement clinker prepared in Example 1 and heavy metal limits for cement clinker in GB / T 30760-2014 Technical Specification for Co-disposal of Solid Wastes in Cement Kilns
[0094]
[0095]
[0096] It can be seen from Table 9 that fly ash contains a large amount of heavy metal ions. The preparation method provided by the present invention can fix the heavy metal ions in the fly ash, and the heavy metal content in the prepared fly ash-doped cement clinker does not exceed the standard limit.
[0097] The results of BCR continuous leaching of the fly ash in Example 1 and the prepared fly ash-doped cement clinker are shown in Table 10.
[0098] Table 10 Results of BCR continuous leaching of fly ash in Example 1 and prepared fly ash-doped cement clinker Unit (mg / kg)
[0099]
[0100] According to the results obtained in Table 10, the percentage contents of heavy metals in different chemical forms in the fly ash and fly ash-doped cement clinker in Example 1 were statistically analyzed, and the percentage distribution diagrams of heavy metals in different chemical forms in the fly ash and fly ash-doped cement clinker in Example 1 were obtained as follows: Figure 1 and Figure 2 shown.
[0101] from Figure 1 and Figure 2 It can be seen that the leaching amount of heavy metals in fly ash is generally high, especially the residual content of heavy metals such as cadmium, manganese, and nickel is only about 20-30%. Most of the heavy metals will be leached in different forms. In addition, the heavy metal content of fly ash itself is also high, and the total amount of heavy metal leaching is also very high. This also shows that if the fly ash is not properly handled, the heavy metals in the fly ash can easily enter the environment through migration, thereby causing a series of environmental problems; the overall content of residual heavy metals in fly ash-doped cement clinker is relatively high, and the residual content is basically around 70%. Compared with the residual content in fly ash, the residual content of basically each heavy metal has increased, even the residual content of manganese in the clinker is about 50%, which is greater than about 30% in fly ash. This also shows that the heavy metals are better fixed in the cement clinker.
[0102] The strength results of the cement mortar in Application Example 1 and the standard strength of the standard "GB175-2007 General Portland Cement" are shown in Table 11.
[0103] Table 11 The strength results of cement mortar in application example 1 and the standard strength of standard "GB175-2007 General Portland Cement"
[0104]
[0105] It can be concluded from Table 11 that the cement mortar prepared from the cement clinker obtained by the preparation method provided by the present invention has a flexural strength of 7.13 MPa and a compressive strength of 46.98 MPa after 28 days of curing, which are higher than the specified strength values and have good mechanical properties.
[0106] The heavy metal leaching amount of cement mortar in Application Example 1 and the leaching limit of mortar specified in the standard "GB30760-2014 Technical Specifications for Co-treatment of Solid Waste in Cement Kilns" are shown in Table 12.
[0107] Table 12 Heavy metal leaching amount of cement mortar in application example 1 and leaching limit of mortar specified in the standard "GB30760-2014 Technical Specification for Co-treatment of Solid Waste in Cement Kilns"
[0108] As(μg / L) Cd(μg / L) Cr(μg / L) Cu(μg / L) Cement mortar 12.63 14.92 52.82 84.34 GB30760-2014 limit 100 30 200 1000 Mn(μg / L) Ni(μg / L) Pb(μg / L) Zn(μg / L) Cement mortar 346.42 89.91 18.32 534.33 GB30760-2014 limit 1000 200 300 1000
[0109] It can be concluded from Table 12 that the heavy metal leaching amount of cement mortar prepared by the fly ash-doped cement clinker prepared by the preparation method provided by the present invention is lower than the prescribed leaching limit, and has a lower metal leaching amount.
[0110] It can be seen from the above examples that the mortar prepared from the fly ash-doped cement clinker obtained by the preparation method provided by the present invention has good mechanical properties and low heavy metal leaching amount.
[0111] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing fly ash-doped cement clinker, comprising the following steps: (1) limestone, converter slag, sandstone and fly ash are mixed and ground to obtain cement raw material; (2) mixing the cement raw meal obtained in step (1) with coal powder and fly ash and calcining the mixture to obtain fly ash-doped cement clinker; The mass of the fly ash in step (2) is 2-3% of the mass of the cement raw material.
2. The preparation method according to claim 1, characterized in that: The mass of the fly ash in step (2) is 2.5-3% of the mass of the cement raw material.
3. The preparation method according to claim 1 or 2, characterized in that: In the step (1), the mass ratio of limestone, converter slag, sandstone and fly ash is (90-93): (2-3): (2-5): (2-3).
4. The preparation method according to claim 3, characterized in that: In the step (1), the mass ratio of limestone, converter slag, sandstone and fly ash is (91-92): (2-2.5): (3-4): (2-2.5).
5. The preparation method according to claim 1 or 2, characterized in that: The mass of the coal powder in step (2) is 7-9% of the mass of the cement raw material.
6. The preparation method according to claim 1, characterized in that: The particle size of the fly ash in step (2) is 12 to 18 μm.
7. The preparation method according to claim 1, characterized in that: The particle size of the coal powder in step (2) is 16 to 22 μm.
8. The preparation method according to claim 1, characterized in that: In the step (2), the calcination temperature is 1400-1480° C., and the calcination time is 30-40 minutes.
9. Cement clinker doped with fly ash prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the fly ash-doped cement clinker according to claim 9 in cement mortar.
Citation Information
Cited By
Method for synergistically and comprehensively treating household garbage incineration fly ash through cement kiln