Ceramic material and application thereof in fuse
By preparing ceramic materials composed of modified fillers and additives, the problem of insufficient strength of the ceramic fuse shell is solved, the mechanical properties of the ceramic material are improved, and its performance under external forces is improved.
Patent Information
- Application Number
- CN202411090904.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-22
AI Technical Summary
At this stage, the shell strength of the ceramic fuse is not high, which affects its production, manufacturing, transportation and fuse characteristics.
A ceramic material composed of modified filler, additive, alumina and zirconia is prepared by specific ball milling and heating treatment methods to form ceramic materials with high mechanical properties, and is produced during the sintering process using modified filler and additives. The bridge effect and silicon carbide structure improve the strength of the material.
It significantly improves the mechanical properties and strength of ceramic materials, can suppress the spread of fracture when subjected to external forces, delay the spread of cracks, and improves the overall performance of ceramic materials.
Smart Images

Figure BDA0004986545950000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ceramic material preparation, and in particular to a ceramic material and an application thereof in a fuse. Background Art
[0002] The function of a fuse is the same as that of a fuse. When the circuit current is abnormal and exceeds its rated current, it will melt and protect the circuit. The fuse will melt the fuse itself and disconnect the circuit from the heat generated by itself. Fuses are widely used in high and low voltage power distribution systems and control systems as well as electrical equipment. As a short circuit and overcurrent protector, it is one of the most commonly used protection devices. As a type of fuse, the fuse of a tubular fuse is installed in the fuse body. At present, the fuse body is mostly made of glass or ceramic. Since the mechanical strength of ceramic is far superior to that of glass, ceramic fuses have gradually become the mainstream. However, alumina ceramics are brittle and have poor toughness, which to a certain extent affects the production, transportation and fusing characteristics of fuses. Summary of the invention
[0003] The purpose of the present invention is to provide a ceramic material and its application in a fuse, which solves the problem that the strength of the ceramic shell of the fuse is low at present.
[0004] The purpose of the present invention can be achieved through the following technical solutions:
[0005] A ceramic material is made by the following steps:
[0006] Step A1: mixing hexagonal boron nitride, urea and deionized water and ball milling for 10-15 hours to obtain amination boron nitride, and mixing graphene oxide, amination boron nitride, dicyclohexylcarbodiimide and toluene uniformly, and reacting for 3-5 hours at a speed of 120-150 r / min and a temperature of 60-70° C. to obtain a modified filler;
[0007] Step A2: Weigh the following raw materials in parts by weight: 2-5 parts of modified filler, 8-10 parts of additives, 90-100 parts of alumina and 10-15 parts of zirconium oxide, ball-mill the raw materials evenly, heat up to 900°C at a heating rate of 5°C / min, and keep warm for 10-15 minutes, heat up to 1400°C at a heating rate of 100°C, and keep warm for 5-10 minutes, heat up to 1600°C at a temperature of 40°C / min, and keep warm for 1-1.5 hours to obtain a ceramic material.
[0008] Furthermore, the dosage ratio of hexagonal boron nitride, urea and deionized water in step A1 is 6 g:180 g:100 mL, and the mass ratio of graphene oxide, amino boron nitride and dicyclohexylcarbodiimide is 1:3:2.
[0009] Further, the density of the aluminum oxide described in step A2 is 3.5 g / cm 3 , the density of zirconium oxide is 6.05g / cm 3 .
[0010] Further, the additive is prepared by the following steps:
[0011] Step B1: Phenyltrimethoxysilane, isopropanol, deionized water and sodium hydroxide are mixed evenly, nitrogen is introduced for protection, and the reaction is carried out for 3-5 hours at a speed of 150-200 r / min and a temperature of 85-90° C., and the temperature is lowered to 20-25° C. and the reaction is carried out for 10-15 hours to obtain intermediate 1. Intermediate 1, triethylamine and DMF are mixed evenly, nitrogen is introduced for protection, methyldichlorosilane is added under stirring at a speed of 120-150 r / min and a temperature of 0° C., and the reaction is carried out for 3-5 hours, and the temperature is raised to 20-25° C. and the reaction is carried out for 20-25 hours to obtain intermediate 2;
[0012] Step B2: Mix intermediate 2, acrylic acid, chloroplatinic acid and toluene uniformly, introduce nitrogen protection, react for 10-15 hours at a speed of 120-150 r / min and a temperature of 80-85° C. to obtain intermediate 3; mix intermediate 3, KH550, dicyclohexylcarbodiimide and toluene uniformly, react for 8-10 hours at a speed of 60-80 r / min and a temperature of 40-50° C. to obtain a modified monomer;
[0013] Step B3: uniformly mix the modified monomer, methyltriethoxysilane, KH570 and ethanol, stir and add deionized water and hydrochloric acid solution at a speed of 120-150r / min and a temperature of 65-70°C, react for 2-3h, add tetrabutyl titanate, continue to react for 2-3h, heat to 120-130°C, keep warm for 3-5h, cool to 50-60°C, add benzophenone and diisopropylbenzene peroxide, react for 1-2h, and prepare the additive.
[0014] Furthermore, the amount ratio of phenyltrimethoxysilane, isopropanol, deionized water and sodium hydroxide described in step B1 is 120mmo l:120mL:3mL:80mmo l, and the mass ratio of intermediate 1, triethylamine and methyldichlorosilane is 12:4.5:3.5.
[0015] Furthermore, the molar ratio of the SiH bond on the intermediate 2 and acrylic acid in step B2 is 1:1, the amount of chloroplatinic acid used is 1‰ of the mass of allyl alcohol, and the molar ratio of the carboxyl group, KH550 and dicyclohexylcarbodiimide on the intermediate 3 is 1:1:1.1.
[0016] Furthermore, the amount ratio of the modified monomer, methyltriethoxysilane, KH570, deionized water, hydrochloric acid solution, tetrabutyl titanate, benzophenone and diisopropylbenzene peroxide described in step B3 is 100 mg: 3 mmol: 1 mmol: 3 mL: 20 mL: 1.5 mmol: 1 mg: 3 mg, and the mass fraction of the hydrochloric acid solution is 10%.
[0017] Beneficial effects of the present invention: A ceramic material prepared by the present invention comprises the following raw materials: modified filler, additives, aluminum oxide and zirconium oxide. The modified filler is treated with urea using hexagonal boron nitride as a raw material so that amino groups are grafted onto the surface to obtain amino-treated boron nitride. The amino-treated boron nitride is reacted with graphene oxide so that the amino groups on the amino-treated boron nitride and the carboxyl groups on the graphene oxide undergo a dehydration reaction to obtain the modified filler.
[0018] The additive is prepared by hydrolyzing phenyltrimethoxysilane as a raw material to form sodium octaphenylcyclotetrasiloxane tetrasilanolate to obtain an intermediate 1, reacting the intermediate 1 with methyldichlorosilane so that the sodium silanolate on the intermediate 1 reacts with the chlorine atom site on the methyldichlorosilane to obtain an intermediate 2, reacting the intermediate 2 with acrylic acid under the action of chloroplatinic acid so that the Si-H bond on the intermediate 2 and the double bond on the acrylic acid are grafted to obtain an intermediate 3, reacting the intermediate 3 with KH550 so that the carboxyl group on the intermediate 3 reacts with the amino group on KH550 to obtain a modified monomer, hydrolyzing and condensing the modified monomer, methyltriethoxysilane, KH570 and tetrabutyl titanate to form an organic silicone resin containing a cage-type silsesquioxane structure and titanium, and further cross-linking under the action of benzophenone and diisopropylbenzene peroxide to obtain an additive.
[0019] This ceramic material has excellent mechanical properties. The additive forms a silicon carbide structure during the high calcination process, and can generate radial tensile stress and tangential compressive stress inside the green body during the sintering process. When subjected to external force, the stress and external force act to cause the material crack to deflect during the diffusion process, and the cracks to bifurcate, consuming part of the fracture energy, thereby inhibiting the diffusion of the fracture. The modified filler and additive can produce a bridging effect in the green body. When the ceramic material is subjected to external force, the modified filler and additive can bridge the disconnected crack surfaces, thereby generating a force to close the crack, thereby improving the strength of the material. DETAILED DESCRIPTION
[0020] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0021] Embodiment 1: A ceramic material is made by the following steps:
[0022] Step A1: mixing hexagonal boron nitride, urea and deionized water and ball milling for 10 hours to obtain amination boron nitride, and mixing graphene oxide, amination boron nitride, dicyclohexylcarbodiimide and toluene uniformly, and reacting at a speed of 120 r / min and a temperature of 60° C. for 3 hours to obtain a modified filler;
[0023] Step A2: Weigh the following raw materials in parts by weight: 2 parts of modified filler, 8 parts of additives, 90 parts of aluminum oxide and 10 parts of zirconium oxide, ball-mill the raw materials evenly, heat up to 900°C at a heating rate of 5°C / min, and keep warm for 10 minutes, heat up to 1400°C at a heating rate of 100°C, and keep warm for 5 minutes, heat up to 1600°C at 40°C / min, and keep warm for 1 hour to obtain a ceramic material.
[0024] The dosage ratio of hexagonal boron nitride, urea and deionized water in step A1 is 6g:180g:100mL, and the mass ratio of graphene oxide, amino boron nitride and dicyclohexylcarbodiimide is 1:3:2.
[0025] The density of the aluminum oxide described in step A2 is 3.5 g / cm 3 , the density of zirconium oxide is 6.05g / cm 3 .
[0026] The additive is prepared by the following steps:
[0027] Step B1: Phenyltrimethoxysilane, isopropanol, deionized water and sodium hydroxide were mixed evenly, nitrogen was introduced for protection, the reaction was carried out at a speed of 150 r / min and a temperature of 85°C for 3 hours, the temperature was lowered to 20°C, and the reaction was carried out for 10 hours to obtain intermediate 1; intermediate 1, triethylamine and DMF were mixed evenly, nitrogen was introduced for protection, methyldichlorosilane was added under stirring at a speed of 120 r / min and a temperature of 0°C, the reaction was carried out for 3 hours, the temperature was raised to 20°C, and the reaction was carried out for 20 hours to obtain intermediate 2;
[0028] Step B2: Intermediate 2, acrylic acid, chloroplatinic acid and toluene are mixed evenly, nitrogen is introduced for protection, and the reaction is carried out for 10 hours at a speed of 120 r / min and a temperature of 80° C. to obtain intermediate 3; intermediate 3, KH550, dicyclohexylcarbodiimide and toluene are mixed evenly, and the reaction is carried out for 8 hours at a speed of 60 r / min and a temperature of 40° C. to obtain a modified monomer;
[0029] Step B3: Evenly mix the modified monomer, methyltriethoxysilane, KH570 and ethanol, stir and add deionized water and hydrochloric acid solution at a speed of 120 r / min and a temperature of 65°C, react for 2 hours, add tetrabutyl titanate, continue to react for 2 hours, heat to 120°C, keep warm for 3 hours, cool to 50°C, add benzophenone and diisopropylbenzene peroxide, react for 1 hour, and prepare the additive.
[0030] The amount ratio of phenyltrimethoxysilane, isopropanol, deionized water and sodium hydroxide described in step B1 is 120mmo l:120mL:3mL:80mmo l, and the mass ratio of intermediate 1, triethylamine and methyldichlorosilane is 12:4.5:3.5.
[0031] The molar ratio of the SiH bond on the intermediate 2 and acrylic acid in step B2 is 1:1, the amount of chloroplatinic acid used is 1‰ of the mass of allyl alcohol, and the molar ratio of the carboxyl group, KH550 and dicyclohexylcarbodiimide on the intermediate 3 is 1:1:1.1.
[0032] The amount ratio of the modified monomer, methyltriethoxysilane, KH570, deionized water, hydrochloric acid solution, tetrabutyl titanate, benzophenone and diisopropylbenzene peroxide described in step B3 is 100 mg: 3 mmol: 1 mmol: 3 mL: 20 mL: 1.5 mmol: 1 mg: 3 mg, and the mass fraction of the hydrochloric acid solution is 10%.
[0033] Embodiment 2: A ceramic material is made by the following steps:
[0034] Step A1: mixing hexagonal boron nitride, urea and deionized water and ball milling for 10 hours to obtain amination boron nitride, and mixing graphene oxide, amination boron nitride, dicyclohexylcarbodiimide and toluene uniformly, and reacting at a speed of 150 r / min and a temperature of 65° C. for 4 hours to obtain a modified filler;
[0035] Step A2: Weigh the following raw materials in parts by weight: 3 parts of modified filler, 9 parts of additives, 95 parts of aluminum oxide and 13 parts of zirconium oxide, ball-mill the raw materials evenly, heat up to 900°C at a heating rate of 5°C / min, and keep warm for 10 minutes, heat up to 1400°C at a heating rate of 100°C, and keep warm for 8 minutes, heat up to 1600°C at 40°C / min, and keep warm for 1.5 hours to obtain a ceramic material.
[0036] The dosage ratio of hexagonal boron nitride, urea and deionized water in step A1 is 6g:180g:100mL, and the mass ratio of graphene oxide, amino boron nitride and dicyclohexylcarbodiimide is 1:3:2.
[0037] The density of the aluminum oxide described in step A2 is 3.5 g / cm 3 , the density of zirconium oxide is 6.05g / cm 3 .
[0038] The additive is prepared by the following steps:
[0039] Step B1: Phenyltrimethoxysilane, isopropanol, deionized water and sodium hydroxide were mixed evenly, nitrogen was introduced for protection, the reaction was carried out at a speed of 150 r / min and a temperature of 90°C for 4 hours, the temperature was lowered to 20°C, and the reaction was carried out for 15 hours to obtain intermediate 1; intermediate 1, triethylamine and DMF were mixed evenly, nitrogen was introduced for protection, methyldichlorosilane was added under stirring at a speed of 120 r / min and a temperature of 0°C, the reaction was carried out for 4 hours, the temperature was raised to 25°C, and the reaction was carried out for 20 hours to obtain intermediate 2;
[0040] Step B2: The intermediate 2, acrylic acid, chloroplatinic acid and toluene are mixed evenly, nitrogen is introduced for protection, and the reaction is carried out for 15 hours at a speed of 150 r / min and a temperature of 80° C. to obtain the intermediate 3; the intermediate 3, KH550, dicyclohexylcarbodiimide and toluene are mixed evenly, and the reaction is carried out for 9 hours at a speed of 60 r / min and a temperature of 45° C. to obtain the modified monomer;
[0041] Step B3: Evenly mix the modified monomer, methyltriethoxysilane, KH570 and ethanol, stir and add deionized water and hydrochloric acid solution at a speed of 120 r / min and a temperature of 68°C, react for 3 hours, add tetrabutyl titanate, continue to react for 2 hours, heat to 125°C, keep warm for 4 hours, cool to 55°C, add benzophenone and diisopropylbenzene peroxide, react for 1.5 hours, and prepare the additive.
[0042] The amount ratio of phenyltrimethoxysilane, isopropanol, deionized water and sodium hydroxide described in step B1 is 120mmo l:120mL:3mL:80mmo l, and the mass ratio of intermediate 1, triethylamine and methyldichlorosilane is 12:4.5:3.5.
[0043] The molar ratio of the SiH bond on the intermediate 2 and acrylic acid in step B2 is 1:1, the amount of chloroplatinic acid used is 1‰ of the mass of allyl alcohol, and the molar ratio of the carboxyl group, KH550 and dicyclohexylcarbodiimide on the intermediate 3 is 1:1:1.1.
[0044] The amount ratio of the modified monomer, methyltriethoxysilane, KH570, deionized water, hydrochloric acid solution, tetrabutyl titanate, benzophenone and diisopropylbenzene peroxide described in step B3 is 100 mg: 3 mmol: 1 mmol: 3 mL: 20 mL: 1.5 mmol: 1 mg: 3 mg, and the mass fraction of the hydrochloric acid solution is 10%.
[0045] Embodiment 3: A ceramic material is made by the following steps:
[0046] Step A1: mixing hexagonal boron nitride, urea and deionized water and ball milling for 15 hours to obtain amination boron nitride, and mixing graphene oxide, amination boron nitride, dicyclohexylcarbodiimide and toluene uniformly, and reacting at a speed of 150 r / min and a temperature of 70° C. for 5 hours to obtain a modified filler;
[0047] Step A2: Weigh the following raw materials in parts by weight: 5 parts of modified filler, 10 parts of additives, 100 parts of alumina and 15 parts of zirconium oxide, ball-mill the raw materials evenly, heat up to 900°C at a heating rate of 5°C / min, and keep warm for 15 minutes, heat up to 1400°C at a heating rate of 100°C, and keep warm for 10 minutes, heat up to 1600°C at 40°C / min, and keep warm for 1.5 hours to obtain a ceramic material.
[0048] The dosage ratio of hexagonal boron nitride, urea and deionized water in step A1 is 6g:180g:100mL, and the mass ratio of graphene oxide, amino boron nitride and dicyclohexylcarbodiimide is 1:3:2.
[0049] The density of the aluminum oxide described in step A2 is 3.5 g / cm 3 , the density of zirconium oxide is 6.05g / cm 3 .
[0050] The additive is prepared by the following steps:
[0051] Step B1: Phenyltrimethoxysilane, isopropanol, deionized water and sodium hydroxide were mixed evenly, nitrogen was introduced for protection, the reaction was carried out at a speed of 200 r / min and a temperature of 90°C for 5 hours, the temperature was lowered to 25°C, and the reaction was carried out for 15 hours to obtain intermediate 1; intermediate 1, triethylamine and DMF were mixed evenly, nitrogen was introduced for protection, methyldichlorosilane was added under stirring at a speed of 150 r / min and a temperature of 0°C, the reaction was carried out for 5 hours, the temperature was raised to 25°C, and the reaction was carried out for 25 hours to obtain intermediate 2;
[0052] Step B2: Intermediate 2, acrylic acid, chloroplatinic acid and toluene are mixed evenly, nitrogen is introduced for protection, and the reaction is carried out for 15 hours at a speed of 150 r / min and a temperature of 85° C. to obtain intermediate 3; intermediate 3, KH550, dicyclohexylcarbodiimide and toluene are mixed evenly, and the reaction is carried out for 10 hours at a speed of 80 r / min and a temperature of 50° C. to obtain a modified monomer;
[0053] Step B3: Evenly mix the modified monomer, methyltriethoxysilane, KH570 and ethanol, stir and add deionized water and hydrochloric acid solution at a speed of 150 r / min and a temperature of 70°C, react for 3 hours, add tetrabutyl titanate, continue to react for 3 hours, heat to 130°C, keep warm for 5 hours, cool to 60°C, add benzophenone and diisopropylbenzene peroxide, react for 2 hours, and prepare the additive.
[0054] The amount ratio of phenyltrimethoxysilane, isopropanol, deionized water and sodium hydroxide described in step B1 is 120mmo l:120mL:3mL:80mmo l, and the mass ratio of intermediate 1, triethylamine and methyldichlorosilane is 12:4.5:3.5.
[0055] The molar ratio of the SiH bond on the intermediate 2 and acrylic acid in step B2 is 1:1, the amount of chloroplatinic acid used is 1‰ of the mass of allyl alcohol, and the molar ratio of the carboxyl group, KH550 and dicyclohexylcarbodiimide on the intermediate 3 is 1:1:1.1.
[0056] The amount ratio of the modified monomer, methyltriethoxysilane, KH570, deionized water, hydrochloric acid solution, tetrabutyl titanate, benzophenone and diisopropylbenzene peroxide described in step B3 is 100 mg: 3 mmol: 1 mmol: 3 mL: 20 mL: 1.5 mmol: 1 mg: 3 mg, and the mass fraction of the hydrochloric acid solution is 10%.
[0057] Comparative Example 1: Compared with Example 1, this comparative example uses graphene instead of the modified filler, and the other steps are the same.
[0058] Comparative Example 2: Compared with Example 1, no modified filler was added in this comparative example, and the remaining steps were the same.
[0059] Comparative Example 3: Compared with Example 1, no additives were added in this comparative example, and the remaining steps were the same.
[0060] Comparative Example 4: Compared with Example 1, this comparative example uses octaphenyl cage silsesquioxane instead of the additive, and the other steps are the same.
[0061] Comparative Example 5: Compared with Example 1, no modified monomer was added in this comparative example, and the remaining steps were the same.
[0062] The ceramic materials obtained in Examples 1-3 and Comparative Examples 1-5 were made into 3mm×4mm×36mm specimens, and the bending strength was tested using a universal testing machine at a span of 30mm and a pressure head loading rate of 0.5mm / min. The ceramic materials were made into 2mm×4mm×22mm specimens, and the fracture toughness was tested at a cut depth of 2mm, a cut width of 0.2mm, a span of 16mm, and a pressure head loading rate of 0.05mm / min. Under a load of 10kg, the pressure was maintained for 10s and the hardness was measured. The test results are shown in the following table.
[0063]
[0064] It can be seen from the above table that the present application has good mechanical strength.
[0065] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. A ceramic material, characterized in that: Made by the following steps: Step A1: mixing hexagonal boron nitride, urea and deionized water and ball milling for 10-15 hours to obtain amination boron nitride, and mixing graphene oxide, amination boron nitride, dicyclohexylcarbodiimide and toluene uniformly, and reacting for 3-5 hours at a speed of 120-150 r / min and a temperature of 60-70° C. to obtain a modified filler; Step A2: Weigh the following raw materials in parts by weight: 2-5 parts of modified filler, 8-10 parts of additives, 90-100 parts of alumina and 10-15 parts of zirconium oxide, ball-mill the raw materials evenly, heat up to 900°C at a heating rate of 5°C / min, and keep warm for 10-15 minutes, heat up to 1400°C at a heating rate of 100°C, and keep warm for 5-10 minutes, heat up to 1600°C at a temperature of 40°C / min, and keep warm for 1-1.5 hours to obtain a ceramic material.
2. A ceramic material according to claim 1, characterized in that: The dosage ratio of hexagonal boron nitride, urea and deionized water in step A1 is 6g:180g:100mL, and the mass ratio of graphene oxide, amino boron nitride and dicyclohexylcarbodiimide is 1:3:
2.
3. A ceramic material according to claim 1, characterized in that: The density of the aluminum oxide described in step A2 is 3.5 g / cm 3 , the density of zirconium oxide is 6.05g / cm 3 .
4. A ceramic material according to claim 1, characterized in that: The additive is prepared by the following steps: Step B1: Phenyltrimethoxysilane, isopropanol, deionized water and sodium hydroxide are mixed evenly, nitrogen is introduced for protection, and the reaction is carried out for 3-5 hours at a speed of 150-200 r / min and a temperature of 85-90° C., and the temperature is lowered to 20-25° C. and the reaction is carried out for 10-15 hours to obtain intermediate 1. Intermediate 1, triethylamine and DMF are mixed evenly, nitrogen is introduced for protection, methyldichlorosilane is added under stirring at a speed of 120-150 r / min and a temperature of 0° C., and the reaction is carried out for 3-5 hours, and the temperature is raised to 20-25° C. and the reaction is carried out for 20-25 hours to obtain intermediate 2; Step B2: Mix intermediate 2, acrylic acid, chloroplatinic acid and toluene uniformly, introduce nitrogen protection, react for 10-15 hours at a speed of 120-150 r / min and a temperature of 80-85° C. to obtain intermediate 3; mix intermediate 3, KH550, dicyclohexylcarbodiimide and toluene uniformly, react for 8-10 hours at a speed of 60-80 r / min and a temperature of 40-50° C. to obtain a modified monomer; Step B3: uniformly mix the modified monomer, methyltriethoxysilane, KH570 and ethanol, stir and add deionized water and hydrochloric acid solution at a speed of 120-150r / min and a temperature of 65-70°C, react for 2-3h, add tetrabutyl titanate, continue to react for 2-3h, heat to 120-130°C, keep warm for 3-5h, cool to 50-60°C, add benzophenone and diisopropylbenzene peroxide, react for 1-2h, and prepare the additive.
5. A ceramic material according to claim 4, characterized in that: The amount ratio of phenyltrimethoxysilane, isopropanol, deionized water and sodium hydroxide described in step B1 is 120mmol:120mL:3mL:80mmol, and the mass ratio of intermediate 1, triethylamine and methyldichlorosilane is 12:4.5:3.
5.
6. A ceramic material according to claim 4, characterized in that: The molar ratio of the Si-H bond on the intermediate 2 and acrylic acid in step B2 is 1:1, the amount of chloroplatinic acid used is 1‰ of the mass of allyl alcohol, and the molar ratio of the carboxyl group, KH550 and dicyclohexylcarbodiimide on the intermediate 3 is 1:1:1.
1.
7. A ceramic material according to claim 4, characterized in that: The amount ratio of the modified monomer, methyltriethoxysilane, KH570, deionized water, hydrochloric acid solution, tetrabutyl titanate, benzophenone and diisopropylbenzene peroxide described in step B3 is 100 mg: 3 mmol: 1 mmol: 3 mL: 20 mL: 1.5 mmol: 1 mg: 3 mg.
8. Use of the ceramic material according to claim 1 in a fuse.
Citation Information
Patent Citations
Silane cross-linking modified ultra-high molecular weight polyethylene fiber preparation method
CN103993479A
Composite ceramic cutter material and method for preparing same
CN106278197A
Photovoltaic photo-thermal dual-curing POE packaging adhesive film and preparation method thereof
CN111117498A
High-strength antistatic release film and preparation method thereof
CN116082689A
Antiskid wear-resistant sole material and preparation method thereof
CN118852831A
Cited By
A2-grade flame-retardant aluminum-plastic panel core material and preparation method thereof
CN121406040A