Bismuth praseodymium iron cobalt titanium ceramic material with ferroelectricity and ferromagnetism and preparation method of bismuth praseodymium iron cobalt titanium ceramic material

By inserting magnetic octahedral groups into the ferroelectric matrix, Bi4PrFe0.5Co0.5Ti3O15 ceramic material was prepared, which solved the problem of low ferromagnetic and ferroelectric coexistence temperatures of multiferrometallic materials at room temperature, and achieved good magnetic properties of the material and simplified preparation processes for new sensors and peptide memories.

CN118993725APending Publication Date: 2024-11-22YANGZHOU UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411089732.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing multiferrous materials have low temperatures of ferromagnetic and ferroelectricity coexisting at room temperature, and the preparation process is complex, resulting in weak magnetic properties and many defects, limiting their application in devices.

Method used

By inserting magnetic octahedral groups into the ferroelectric matrix, PrFe0.5Co0.5O3 and Bi4Ti3O12 powders were prepared by hydrothermal method, and then annealing and sintering were performed to prepare Bi4PrFe0.5Co0.5Ti3O15 ceramics with ferroelectricity and ferromagneticity were prepared. Material.

Benefits of technology

The good ferroelectricity and ferromagnetic coexistence of bismuth praseodymium cobalt titanium ceramic materials at room temperature is achieved, the preparation process is simplified, the sample defect concentration is reduced, and the magnetic performance is improved. It is suitable for use in new sensors and peptide memories.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993725A_ABST
    Figure CN118993725A_ABST
Patent Text Reader

Abstract

The invention discloses a bismuth, praseodymium, iron, cobalt and titanium ceramic material with ferroelectricity and ferromagnetism. The structural formula of the bismuth, praseodymium, iron, cobalt and titanium ceramic material is Bi < 4 > PrFe < 0.5 > Co < 0.5 > Ti < 3 > O < 15 >. The preparation method comprises the following steps: respectively preparing PrFe0. 5Co0. 5O3 powder and Bi4Ti3O12 powder by adopting a hydrothermal method, mixing the two materials according to a molar ratio of 1: 1, adding absolute ethyl alcohol, grinding and dispersing, carrying out primary annealing reaction in a muffle furnace, cooling, adding absolute ethyl alcohol again, grinding and dispersing, carrying out secondary annealing reaction in the muffle furnace, and cooling, tabletting and sintering after the reaction is finished, thereby obtaining the PrFe0. 5Co0. 5O3 / Bi4Ti3O12 composite material. Compared with an existing Bi5FeTi3O15 material, the ceramic material has the advantages that the Bi content in a sample is reduced, the defect concentration of the sample can be effectively reduced, the multiferroic property of the material is improved, and the ceramic material has good ferroelectricity and ferromagnetism at the room temperature and is particularly suitable for being applied to the fields of novel sensors, polypeptide memories and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a bismuth-praseodymium-iron-cobalt-titanium ceramic material with ferroelectricity and ferromagnetism and a preparation method thereof, belonging to the technical field of ceramic materials. Background Art

[0002] Single-phase multiferroic materials (MFs) have great application potential in magnetic sensors, data storage devices and digital memories due to their coexistence of ferromagnetism, ferroelectricity and ferroelasticity, and have attracted extensive attention. Among the many MFs studied in the past few decades, we found that ferromagnetism and ferroelectricity are mutually exclusive, and multiferroic materials basically do not exist in nature. At the same time, the coexistence temperature of ferromagnetism and ferroelectricity of many materials is below room temperature (RT), which seriously limits the application of these materials in devices (such as new sensors, peptide memories, etc.).

[0003] Aurivillius material with bismuth layer structure (its general structural formula is: (Bi2O2) 2+ (A n-1 B n O 3n+1 ) 2- (A = Sr, Ca, La, Bi, Pb, etc.; B = Ti, Fe, Co, Ni, etc.; n is the number of perovskite layers)) has been widely studied as a single-phase multiferroic material with application prospects. 15 (BFTO) is a four-layer bismuth perovskite Aurivillius structure oxide, which has ferroelectricity and weak ferromagnetism at room temperature. It has good ferroelectric properties and a relatively high Curie temperature, but its magnetism is weak and the preparation process is complicated. 12 ) is a typical Aurivillius phase ferroelectric material, which has large ferroelectric spontaneous polarization, non-volatility and high Curie temperature and can be used in non-volatile memory. Studies have shown that Bi ions are easily volatilized during high-temperature sintering, resulting in defects such as oxygen vacancies. The defects in the sample will cause increased leakage current and ferroelectric domain pinning, which will lead to problems such as reduced remanent magnetic polarization and poor fatigue resistance.

[0004] Perovskite bismuth ferrite BiFeO3 (BFO), as a single-phase magnetoelectric multiferroic, has ferroelectricity and a Curie temperature T C ≈830℃, antiferromagnetic, Neel temperature T N=310℃, it may be the only material that exhibits spontaneous ferroelectricity and magnetic order above room temperature. However, the magnetization intensity and magnetoelectric effect of BFO are relatively weak and cannot meet the needs of practical applications. Therefore, improving its magnetic properties is the key to solving this problem. Ion substitution is a common method to induce ferromagnetism in BFO. Current research mainly focuses on doping different ions in BFO to obtain enhanced ferromagnetism, such as doping with rare earth ions (La, Nd, Sm, etc.) at the A site in BFO (i.e., the Bi site in BFO), or doping with transition metal ions (Mn, Ti, Cr, Co, Sc, etc.) at the B site in BFO (i.e., the Fe site in BFO). The inventors intend to use Pr to replace the Bi ion at the A site. It is reported that PrFeO3 has an orthorhombic perovskite structure with a tolerance factor of 0.8265, where Pr 3+ The ion occupies the A site of the dodecahedron, Fe 3+ The ions occupy the octahedral B site, which has a distorted FeO6 octahedron. When studying the B-site substitution of BFO samples, the equivalent magnetic ion Co 3+ ions to replace part of the Fe 3+ After doping, it was found that the magnetic properties of the sample were improved and when the content of Co and Fe was 1:1, the residual magnetization intensity reached the maximum value, which may be due to the existence of local Fe-O-Co coupling.

[0005] In summary, the present inventor intends to achieve the coexistence of ferromagnetism and ferroelectricity by inserting magnetic octahedral groups into the ferroelectric matrix. Based on this idea, the present invention uses doped PrFe 0.5 Co 0.5 O3 powder material intercalated into Bi4Ti3O 12 Powder, prepared Bi4PrFe with good magnetic properties 0.5 Co 0.5 Ti3O 15 Ceramic materials, improved Bi5FeTi3O 15 Multiferroic properties of materials. Summary of the invention

[0006] The object of the present invention is to solve the deficiencies of the above-mentioned background technology and provide a bismuth-praseodymium-iron-cobalt-titanium ceramic material with ferroelectricity and ferromagnetism and a preparation method thereof. The bismuth-praseodymium-iron-cobalt-titanium ceramic material has good ferroelectricity and ferromagnetism at room temperature.

[0007] In order to achieve the above object, the present invention adopts the following technical solution:

[0008] A bismuth-praseodymium-iron-cobalt-titanium ceramic material having ferroelectricity and ferromagnetism, wherein the structural formula of the ceramic material is: Bi4PrFe 0.5 Co 0.5 Ti3O 15 .

[0009] The method for preparing the bismuth-praseodymium-iron-cobalt-titanium ceramic material having ferroelectricity and ferromagnetism comprises the following steps:

[0010] (1) PrFe was prepared by hydrothermal method using praseodymium nitrate hexahydrate, cobalt nitrate hexahydrate, iron nitrate nonahydrate and sodium hydroxide as raw materials. 0.5 Co 0.5 O3 powder;

[0011] (2) Bi4Ti3O was prepared by hydrothermal method using bismuth nitrate pentahydrate, nitric acid, tetrabutyl titanate and sodium hydroxide as raw materials. 12 powder;

[0012] (3) PrFe 0.5 Co 0.5 O3 powder and Bi4Ti3O 12 The powders are mixed evenly, added with anhydrous ethanol to grind and disperse, and then put into a muffle furnace for a first annealing reaction. After cooling, anhydrous ethanol is added again to grind and disperse, and then put into a muffle furnace for a second annealing reaction. After the end, the powders are cooled, pressed into sheets, and finally sintered to obtain a bismuth-praseodymium-iron-cobalt-titanium ceramic material with ferroelectricity and ferromagnetism.

[0013] Further, in step (1), the hydrothermal method is used to prepare PrFe 0.5 Co 0.5 O3 powder method: According to the structural formula PrFe 0.5 Co 0.5 Weigh praseodymium nitrate hexahydrate, iron nitrate nonahydrate and cobalt nitrate hexahydrate in a stoichiometric ratio in O3, mix and dissolve in deionized water, then drop sodium hydroxide solution, stir to form a turbid liquid, transfer to a reactor and react at 155-165°C for 12-16h, then cool to room temperature, wash the obtained product, dry it, grind it, and then place it in a muffle furnace at 650-750°C for 3-5h to obtain PrFe 0.5 Co 0.5 O3 powder.

[0014] Further, in step (2), the hydrothermal method is used to prepare Bi4Ti3O 12 Powder method: According to the structural formula Bi4Ti3O 12 Weigh bismuth nitrate pentahydrate and tetrabutyl titanate in a stoichiometric ratio, add them to deionized water, add nitric acid to dissolve them, then add sodium hydroxide solution dropwise, stir to form a turbid liquid, transfer to a reactor, react at 200-220°C for 40-50h, then cool to room temperature, take out, wash and dry to obtain Bi4Ti3O 12 powder.

[0015] Further, in step (3), the PrFe0.5 Co 0.5 O3 powder and Bi4Ti3O 12 The molar ratio of the powders was 1:1.

[0016] Furthermore, in step (3), the temperature of the first annealing reaction is 600-700° C., and the time is 3-5 hours.

[0017] Furthermore, in step (3), the temperature of the second annealing reaction is 750-850° C. and the time is 3-5 hours.

[0018] Furthermore, in step (3), the sintering temperature is 900-1000° C. and the sintering time is 3-5 hours.

[0019] Beneficial effects of the present invention:

[0020] 1) The present invention provides a bismuth-praseodymium-iron-cobalt-titanium ceramic material having ferroelectricity and ferromagnetism. First, BTO and PrFe are prepared by a hydrothermal method. 0.5 Co 0.5 O3 two perovskite materials, and then these two perovskite materials are mixed in a molar ratio of 1:1 to synthesize Bi4PrFe 0.5 Co 0.5 Ti3O 15 (BPFCTO) ceramic material, which has good ferroelectricity and ferromagnetism at room temperature, is particularly suitable for application in new sensors, polypeptide storage and other fields.

[0021] 2) The bismuth-praseodymium-iron-cobalt-titanium ceramic material of the present invention has a simple preparation process, simple raw materials and low preparation temperature.

[0022] 3) Compared with the existing Bi5FeTi3O 15 The bismuth-praseodymium-iron-cobalt-titanium ceramic material of the present invention reduces the Bi content in the sample, can effectively reduce the defect concentration of the sample, and improves the Bi5FeTi3O 15 Multiferroic properties of materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is the XRD pattern of the bismuth-praseodymium-iron-cobalt-titanium ceramic material prepared in Example 1;

[0024] Figure 2 This is the VSM diagram of the bismuth, praseodymium, iron, cobalt and titanium ceramic material prepared in Example 1. DETAILED DESCRIPTION

[0025] The technical solution of the present invention is clearly and completely described below in conjunction with the accompanying drawings and specific embodiments.

[0026] It should be noted that in the following embodiments, praseodymium nitrate hexahydrate (Pr(NO3)3·6H2O), ferric nitrate nonahydrate (Fe(NO3)3·9H2O), cobalt nitrate hexahydrate (Co(NO3)·6H2O), sodium hydroxide (NaOH), bismuth nitrate pentahydrate (Bi(NO3)3·5H2O), tetrabutyl titanate (Ti(C4H9O)4), and nitric acid (HNO3) were all purchased from Shanghai Chemical Reagent Company, but are not limited to this.

[0027] Example 1

[0028] A method for preparing a bismuth-praseodymium-iron-cobalt-titanium ceramic material having ferroelectricity and ferromagnetism comprises the following steps:

[0029] (1) Preparation of PrFe by hydrothermal method 0.5 Co 0.5 O3 powder: According to the structural formula PrFe 0.5 Co 0.5 O3 in a stoichiometric ratio, weigh 1.7576g of praseodymium nitrate hexahydrate, 0.8203g of ferric nitrate nonahydrate and 0.5879g of cobalt nitrate hexahydrate, mix and dissolve in 30mL of deionized water, then drop sodium hydroxide solution (containing 0.5g of sodium hydroxide), stir to form a turbid liquid, transfer to a reactor, react at 160°C for 15h, then cool to room temperature, wash the obtained product with anhydrous ethanol and deionized water three times each, dry at 70°C for 12h, grind, and then place in a muffle furnace at 700°C for 4h to obtain PrFe 0.5 Co 0.5 O3 powder (PFCO for short).

[0030] (2) Preparation of Bi4Ti3O by hydrothermal method 12 Powder: According to the structural formula Bi4Ti3O 12 According to the stoichiometric ratio in the reaction mixture, 2.9398 g of bismuth nitrate pentahydrate and 1.5629 g of tetrabutyl titanate (Ti(C4H9O)4) were weighed and added to deionized water, 5.8163 g of nitric acid was added to form a solution, and a sodium hydroxide solution (containing 6.25 g of sodium hydroxide) was added dropwise, stirred to form a turbid liquid, and then transferred to a reactor, reacted at 205°C for 48 hours, then cooled to room temperature, taken out, washed with anhydrous ethanol and deionized water three times each, and dried at 70°C for 12 hours to obtain Bi4Ti3O 12 Powder (BTO for short).

[0031] (3) 0.2462g PrFe 0.5 Co 0.5 O3 powder and 1.1716 g Bi4Ti3O 12The powders were mixed evenly, added with anhydrous ethanol and ground and dispersed for 30 minutes, then placed in a muffle furnace, annealed at 660°C for 4 hours, cooled, added with anhydrous ethanol again, ground and dispersed for 30 minutes, then placed in a muffle furnace, annealed at 800°C for 4 hours, cooled and pressed into sheets, and finally placed in a muffle furnace and sintered at 960°C for 4 hours to obtain a bismuth-praseodymium-iron-cobalt-titanium ceramic material with ferroelectricity and ferromagnetism. 0.5 Co 0.5 Ti3O 15 (abbreviated as BPFCTO).

[0032] Comparative Example 1

[0033] Preparation of Bi5FeTi3O 15 A method for producing a ceramic material, comprising the steps of:

[0034] (1) Bi2O3 and TiO2 powders were mixed in a stoichiometric ratio (15 wt% Bi2O3 was added to compensate for the volatilization of Bi2O3 during sintering) to obtain an oxide mixture, anhydrous ethanol was added to the oxide mixture and ball-milled for 24 h, and then calcined at 760, 780 and 800 °C for 8, 16 and 24 h three times respectively (the reactants were re-ground after each calcination) to obtain BTO powder;

[0035] (2) The obtained BTO powder was mixed with Fe2O3 and Bi2O3 reagents according to the stoichiometric ratio (BTO:Fe2O3:Bi2O3=1:1 / 2:1 / 2). Finally, the pretreated powder was pressed into pellets and sintered in air at 825°C for 4 h to obtain Bi5FeTi3O 15 Sample (referred to as BFTO).

[0036] Figure 1 The XRD pattern of the bismuth-praseodymium-iron-cobalt-titanium ceramic material prepared in Example 1 is shown in FIG. Figure 1 It can be seen that PFCO, BTO and BPFCTO are all perovskite phases, and no secondary phase is found. The lattice constants (a, b, c) of samples PFCO, BTO and BPFCTO are calculated by related diffraction peaks: (0.5409, 0.5501, 0.7684), (0.5440, 0.5413, 3.2395) and (0.5528, 0.5506, 4.0430), respectively.

[0037] Figure 2 This is the VSM diagram of the bismuth-praseodymium-iron-cobalt-titanium ceramic material prepared in Example 1. According to the literature, the undoped Bi5FeTi3O 15 The magnetic curve of (BFTO) material at room temperature is approximately linear, showing a paramagnetic state and 2M r As small as 2.7×10 -6emu / g. from Figure 2 It can be seen that both PFCO and BPFCTO samples have typical ferromagnetic loops at room temperature, especially the 2M loop of sample BPFCTO. s ~3.61emu / g, 2M r It is 0.88emu / g, which is a significant improvement in magnetic properties compared to the BFTO sample.

Claims

1. A bismuth-praseodymium-iron-cobalt-titanium ceramic material having ferroelectricity and ferromagnetism, characterized in that: The structural formula of the ceramic material is: Bi4PrFe 0.5 Co 0.5 Ti3O 15 .

2. The method for preparing the bismuth-praseodymium-iron-cobalt-titanium ceramic material having ferroelectricity and ferromagnetism according to claim 1, characterized in that: The steps include: (1) PrFe was prepared by hydrothermal method using praseodymium nitrate hexahydrate, cobalt nitrate hexahydrate, iron nitrate nonahydrate and sodium hydroxide as raw materials. 0.5 Co 0.5 O3 powder; (2) Bi4Ti3O was prepared by hydrothermal method using bismuth nitrate pentahydrate, nitric acid, tetrabutyl titanate and sodium hydroxide as raw materials. 12 powder; (3) PrFe 0.5 Co 0.5 O3 powder and Bi4Ti3O 12 The powders are mixed evenly, added with anhydrous ethanol to grind and disperse, and then put into a muffle furnace for a first annealing reaction. After cooling, anhydrous ethanol is added again to grind and disperse, and then put into a muffle furnace for a second annealing reaction. After the end, the powders are cooled, pressed into sheets, and finally sintered to obtain a bismuth-praseodymium-iron-cobalt-titanium ceramic material with ferroelectricity and ferromagnetism.

3. The method for preparing the bismuth-praseodymium-iron-cobalt-titanium ceramic material having ferroelectricity and ferromagnetism as claimed in claim 2, characterized in that: In step (1), the hydrothermal method is used to prepare PrFe 0.5 Co 0.5 O3 powder method: According to the structural formula PrFe 0.5 Co 0.5 Weigh praseodymium nitrate hexahydrate, iron nitrate nonahydrate and cobalt nitrate hexahydrate in a stoichiometric ratio in O3, mix and dissolve in deionized water, then drop sodium hydroxide solution, stir to form a turbid liquid, transfer to a reactor and react at 155-165°C for 12-16h, then cool to room temperature, wash the obtained product, dry it, grind it, and then place it in a muffle furnace at 650-750°C for 3-5h to obtain PrFe 0.5 Co 0.5 O3 powder.

4. The method for preparing the bismuth-praseodymium-iron-cobalt-titanium ceramic material having ferroelectricity and ferromagnetism as claimed in claim 2, characterized in that: In step (2), the hydrothermal method is used to prepare Bi4Ti3O 12 Powder method: According to the structural formula Bi4Ti3O 12 Weigh bismuth nitrate pentahydrate and tetrabutyl titanate in a stoichiometric ratio, add them to deionized water, add nitric acid to dissolve them, then add sodium hydroxide solution dropwise, stir to form a turbid liquid, transfer to a reactor, react at 200-220°C for 40-50h, then cool to room temperature, take out, wash and dry to obtain Bi4Ti3O 12 powder.

5. The method for preparing the bismuth-praseodymium-iron-cobalt-titanium ceramic material having ferroelectricity and ferromagnetism as claimed in claim 2, characterized in that: In step (3), the PrFe 0.5 Co 0.5 O3 powder and Bi4Ti3O 12 The molar ratio of the powders was 1:

1.

6. The method for preparing the bismuth-praseodymium-iron-cobalt-titanium ceramic material having ferroelectricity and ferromagnetism as claimed in claim 2, characterized in that: In step (3), the temperature of the first annealing reaction is 600-700° C. and the time is 3-5 hours.

7. The method for preparing the bismuth-praseodymium-iron-cobalt-titanium ceramic material having ferroelectricity and ferromagnetism as claimed in claim 2, characterized in that: In step (3), the temperature of the second annealing reaction is 750-850° C. and the time is 3-5 hours.

8. The method for preparing the bismuth-praseodymium-iron-cobalt-titanium ceramic material having ferroelectricity and ferromagnetism according to any one of claims 2 to 7, characterized in that: In step (3), the sintering temperature is 900-1000° C. and the sintering time is 3-5 hours.

Citation Information

Patent Citations

  • Layered structure ferrotitanium lanthanum bismuth cobaltate ceramic with multiferroic and preparation method thereof

    CN101704669A

  • Preparation method of bismuth ferrotitanium cobaltate powder

    CN110204330A

  • Method for preparing EuCo0. 5Fe0. 5O3 ceramic powder by adopting hydrothermal method

    CN118206370A