Preparation method of Ti2Nb10O29 powder

The preparation of Ti2Nb10O29 powder by one-step calcination method solves the shortcomings of the negative electrode materials of lithium-ion batteries in high-rate charging and discharging and safety, simplifies the process flow, improves the electrochemical performance and safety of the battery, and is suitable for high-performance electric vehicles and Large-scale energy storage system.

CN118993731AActive Publication Date: 2024-11-22SHANDONG UNIV OF TECH

Patent Information

Application Number
CN202411227990.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-22
Estimated Expiration
2044-09-03

AI Technical Summary

Technical Problem

Existing lithium-ion battery anode materials have shortcomings in high-rate charging and discharging, safety and long-term stability. In particular, graphite and silicon materials are prone to lithium dendrites during charging and discharging, internal short circuits and thermal runaway, and high temperatures. The calcination process is complex, affecting battery performance and safety.

Method used

Using (Ti0.2Nb0.8)C micron powder as raw material, high-purity Ti2Nb10O29 powder was prepared by one-step calcination method, simplifying the process flow, shortening the experimental cycle, and using the face-centered cubic crystal structure of carbides to accelerate the oxidation reaction and improve the reaction Efficiency and uniformity.

Benefits of technology

It significantly improves the electrochemical performance and safety of lithium-ion batteries, meets the needs of high-performance lithium-ion batteries, simplifies the preparation process, is suitable for large-scale production, and improves the cycle stability and safety of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention provides a method for preparing titanium niobate (Ti2Nb10O29, called TNO for short) powder, and belongs to the technical field of ceramic powder preparation. The preparation method comprises the following steps: heating (Ti0. 2Nb0. 8) C micron powder serving as a raw material to 800-1300 DEG C in an air atmosphere at a heating rate of 2-10 DEG C / min by adopting a one-step calcination method, oxidizing for 1-5 hours, and cooling to room temperature along with a furnace to obtain the TNO powder. According to the method, the preparation process is simplified, and the production efficiency is improved. A high-performance negative electrode material is provided for a lithium ion battery, and challenges in the aspects of high-rate charging and discharging, high safety and long-period stability are effectively solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for preparing a negative electrode material for a lithium ion battery, in particular to a Ti2Nb 10 O 29 The powder preparation method is used to increase the charging speed of lithium-ion batteries, enhance battery safety and extend battery life. Background Art

[0002] As a key electrochemical energy storage device, lithium-ion batteries (LIBs) have been used in a wide range of fields from portable devices to electric vehicles to power grid systems due to their advantages such as high energy density, no memory effect, environmental friendliness and durability. However, the technology also faces some challenges in its development, such as the need to improve charging speed, extend service life and enhance battery safety. In particular, in high-performance electric vehicles and large-scale energy storage systems, high-energy-density LIBs are required to fit in limited space and enable long-term operation of electric vehicles. These challenges have become the main bottleneck. The development of high-performance anode materials will help promote the advancement of lithium-ion battery technology and broaden its application range. At present, graphite has dominated the anode material market for commercial lithium-ion batteries because of its easy lithium-ion insertion / extraction, high theoretical capacity (372 mAh / g), long cycle life and low cost. However, its low working potential (about 0.02 V vs. Li / Li + ) causes the formation of lithium dendrites during the discharge / charge cycle, which may pierce the separator, causing internal short circuits and thermal runaway, which may cause fire or even explosion, increasing safety risks. At the same time, the passivated solid electrolyte interface (SEI) layer on the surface of carbon materials damages the rate capacity of LIBs in the electrochemical process and reduces the coulombic efficiency. In addition, the low ionic conductivity of graphite hinders the ability of lithium-ion batteries to achieve ultra-fast charging (its capacity is less than 100 mAh / g at a current density of 2C). In addition, silicon (Si) has abundant resources and a theoretical capacity much higher than graphite (4200 mAh g -1 ) and a moderate lithium insertion potential (<0.5 V vs. Li / Li +) and low cost, and is another major commercial lithium-ion battery negative electrode material. However, silicon undergoes significant volume expansion during the electrochemical cycle, about 300%-400% of the original silicon particles. This volume change can cause silicon particles to be easily pulverized and broken during the cycle, affecting the integrity of the electrode structure. Due to the repeated volume expansion and contraction, the solid electrolyte interface (SEI) film on the silicon negative electrode is easily broken and reformed, resulting in irreversible capacity loss and reduced battery cycle life, seriously affecting the battery's charge and discharge capacity and stability. Therefore, there is an urgent need to develop new lithium-ion battery negative electrode materials with reasonable operating voltage, high theoretical capacity, excellent rate performance and good safety.

[0003] Ti2Nb 10 O 29 (TNO) is a titanium niobate with a complex structure and is regarded as a potential negative electrode material for fast-charging lithium-ion batteries; it has attracted widespread attention. TNO belongs to the monoclinic Wadsley-Roth shear structure with lattice constants of a = 15.57 Å, b = 3.814 Å, c = 20.54 Å, α=90°, β=113.7° and γ=90°. The crystal structure is formed by orderly stacking of 3× 4 × ∞ ReO3 type structural units. These structures are composed of corner-sharing and edge-sharing NbO6 and TiO6 octahedra, which extend infinitely along the b-axis to form a columnar structure, and adjacent structural units on the same horizontal plane are connected by edge sharing. In this structure, Ti 4+ and Nb 5+ The ions are randomly arranged on the octahedral sites with an atomic ratio of 1:5, forming an open tunnel-type interstitial space in the

[010] direction. This space allows lithium ions to be inserted and removed without causing structural collapse. This allows TNO to maintain good structural stability at high current density, reducing the formation of SEI (solid electrolyte interface) layer, thereby improving cycle stability. In addition, during the electrochemical reaction, TNO can pass through Nb 5+ / Nb 4+ / Nb 3+ and Ti 4+ / Ti 3+ The multi-electron reaction of TNO can provide a higher theoretical lithium storage capacity than graphite (396 mAh / g). It is worth noting that TNO has a higher lithium ion (de)insertion working potential (1.6 V vs. Li / Li + ), which can effectively prevent the formation of lithium dendrites and the decomposition of electrolyte, thereby improving the safety and cycle stability of the battery.

[0004] In conclusion, Ti2Nb 10 O29 With excellent theoretical capacity, high operating voltage and good structural stability, it has become a promising negative electrode material for lithium-ion batteries and has been explored more deeply. The current processes for preparing TNO materials include solid-phase synthesis, solvothermal method and electrospinning method. Among them, the solid-phase reaction method based on TiO2 and Nb2O5 powder as raw materials is used for large-scale synthesis of Ti2Nb 10 O 29 Negative electrode materials are the most commonly used preparation method. For example, Wu et al. 10 O 29 TiO2 and Nb2O5 powders were mixed in a stoichiometric ratio and heated to 1100°C in air at a heating rate of 5°C / min and kept at this temperature for 36 hours. After cooling in the furnace, Ti2Nb 10 O 29 The product exhibits good rate performance, with an initial coulombic efficiency of 92% at a current density of 0.1C in the potential range of 1.0 to 2.5 V. At current densities of 2C and 10C, reversible capacities of 210 mAh / g and 133 mAh / g were obtained. 10 O 29 The stoichiometric TiO2 and Nb2O5 powders were mixed by high-energy ball milling and calcined at 1000°C for 10 hours in air atmosphere, and then naturally cooled to room temperature. The electrochemical results showed that the prepared Ti2Nb 10 O 29 The material has good stability in high-rate discharge-charge cycles; at a current density of 10C, after 800 cycles, its reversible capacity can still be maintained at 144 mAh / g, and the capacity retention rate reaches 68%. The solid-phase reaction synthesis process is very simple, but the long-term high-temperature calcination process (above 1000°C and more than 10 hours) will cause the TNO grains to grow rapidly (greater than 20 microns), which is not conducive to achieving excellent electrochemical performance. Liu et al. in the paper "Mesoporous Ti2Nb 10 O 29Ti2Nb was prepared by solvothermal method and subsequent calcination. 10 O 29 Microspheres. Titanium tetraisopropylate, niobium pentachloride, isopropanol and glycerol raw materials were mixed evenly in proportion and transferred to a polytetrafluoroethylene-lined high-pressure reactor. After a solvothermal reaction at 180°C for 24 hours. The obtained product was centrifuged, washed, dried and calcined at 900°C in an air atmosphere for 10 hours to obtain microspheres with a diameter of 1-2μm assembled from TNO nanoparticles. The product exhibited excellent electrochemical properties. At different current densities (1, 5, 10, 20 and 30C), the first discharge capacity of TNO microspheres reached 268.9, 218.5, 205.3, 180.5 and 158.1mAh / g, respectively; and at a current density of 10C, after 500 cycles, its capacity could still be maintained at 173.5mAh / g, indicating that it has excellent cycle stability. Deng et al. reported in the paper "One-dimensional Ti2Nb 10 O 29 TNO nanowires were prepared by electrospinning. Citric acid, tetrabutyl titanate, distilled water, polyvinyl pyrrolidone (PVP) and niobium oxalate were added to ethanol in sequence. After being stirred and fully mixed, the precursor was transferred to a disposable syringe. A constant voltage of 12 kV was used and the distance between the needle tip and the stainless steel collector was set to 15 cm. The electrospinning product was heated to 800°C at a heating rate of 5°C / min in an air atmosphere and kept warm for 10 hours to obtain TNO nanowires. The product showed excellent rate performance, that is, at current densities of 0.5, 1, 2, 3, 4 and 5C, its capacity was 251.3, 240.3, 221.8, 205.3, 188.1 and 174.5, respectively. mAh / g. In addition, at a current density of 12C, after 900 cycles, its capacity was maintained at 85.90%, indicating that the TNO nanowires have excellent stability. However, the above studies show that both solvothermal and electrospinning methods require additional subsequent high-temperature calcination processes, and the synthesis route is relatively complicated.

[0005] Aiming at the shortcomings of existing lithium-ion battery negative electrode materials in high rate charge and discharge, high safety requirements and long cycle stability, the present invention proposes a new high-performance negative electrode material Ti2Nb 10 O 29Powder preparation method. Using (Ti 0.2 Nb 0.8 )C micron powder is used as raw material, and the present invention can prepare high-purity Ti2Nb by a one-step calcination method. 10 O 29 This method simplifies the preparation process and shortens the experimental cycle. It is very suitable for lithium-ion batteries in high-performance electric vehicles and large-scale energy storage systems. It can significantly improve the performance and safety of batteries and meet the needs of modern high-end energy equipment. Summary of the invention

[0006] In order to solve the limitations of existing lithium-ion battery negative electrode materials in high-rate charge and discharge, high safety requirements and long-cycle stability, the present invention proposes a new high-performance negative electrode material Ti2Nb 10 O 29 (TNO) powder preparation method. This method uses (Ti 0.2 Nb 0.8 )C powder as raw material, through a one-step calcination method, high-purity TNO powder was successfully prepared. Its technical route includes the following two main steps:

[0007] Ti2Nb 10 O 29 Powder preparation process: Select (Ti 0.2 Nb 0.8 )C micron powder is used as raw material. First, the carbide precursor is placed in a furnace and heated to 800~1300℃ at a heating rate of 2~10℃ / min in an air atmosphere, and an oxidation treatment is performed at this temperature for 1~5 hours. After the oxidation reaction is completed, it is cooled to room temperature with the furnace to obtain high-purity TNO powder.

[0008] (Ti 0.2 Nb 0.8 )C micron powder preparation: TiC, NbC and Co powder are used as raw materials. First, weigh TiC and NbC powders in a molar ratio of 1:4. Then, weigh these carbide powders and Co powder in a mass ratio of 7:3 and mix them evenly. After the mixed powder is pre-pressed into shape through a mold, it is transferred to a furnace. In an argon protective atmosphere, the temperature is heated to 1500°C at a heating rate of 8°C / min and kept warm for 8 hours. After the reaction is completed, the product is allowed to cool naturally to room temperature with the furnace, and (Ti 0.2 Nb 0.8 )C / Co based composite material block. After that, the composite material block is immersed in nitric acid solution to corrode and dissolve the Co alloy matrix. After the corrosion is completed, it is filtered, then repeatedly washed with deionized water and alcohol, and dried to finally obtain (Ti 0.2 Nb 0.8 )C micron powder.

[0009] The working principle of the present invention is based on (Ti 0.2 Nb 0.8 )C powder is used as raw material. The carbide has a face-centered cubic (FCC) crystal structure (space group Fm3 ̅m, number 225). In this structure, carbon atoms are located at the face center of the cube, while Ti and Nb atoms are randomly and evenly distributed at the vertices and body center of the cube according to the molar ratio. This crystal structure is conducive to the uniform and proportional diffusion of Ti and Nb. During the high-temperature oxidation process, oxygen molecules quickly penetrate into the crystal structure and react with Ti and Nb atoms to form high-purity Ti2Nb 10 O 29 Oxide. The distance between Ti and Nb atoms in the lattice is several atoms, which effectively reduces the required diffusion distance and accelerates their reaction rate with oxygen. Compared with the traditional solid phase synthesis of Ti2Nb through TiO2 and Nb2O5 10 O 29 Compared with the conventional method, the method of the present invention has obvious advantages in raw material uniformity and reaction efficiency. In the conventional method, the uneven mixing of raw materials leads to a large diffusion distance of Ti and Nb atoms, requiring a higher reaction temperature and a longer holding time, and easily leads to low product purity and unevenness.

[0010] The present invention uses (Ti 0.2 Nb 0.8 )C powder as raw material fundamentally ensures the uniformity of the reaction environment. During the oxidation process, the diffusion path required for Ti and Nb atoms is short, and these atoms can participate in the oxidation reaction in equal proportions and uniformly. This feature effectively reduces the temperature and time required to prepare high-purity TNO powder, and significantly improves the uniformity and efficiency of the reaction. The TNO powder obtained has excellent electrochemical properties and meets the stringent requirements of high-performance lithium-ion battery negative electrode materials. In addition, the preparation process of the present invention is simple to operate, has a short experimental cycle, and is suitable for large-scale production applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 The Ti2Nb prepared in Example 1 10 O 29 XRD pattern of powder.

[0012] Figure 2 The Ti2Nb prepared in Example 1 10 O 29 SEM image of powder.

[0013] Figure 3 The Ti2Nb prepared in Example 1 10 O 29EDS point analysis spectrum of powder.

[0014] Figure 4 The Ti2Nb prepared in Example 2 10 O 29 XRD pattern of powder.

[0015] Figure 5 The Ti2Nb prepared in Example 2 10 O 29 SEM image of powder.

[0016] Figure 6 The Ti2Nb prepared in Example 3 10 O 29 XRD pattern of powder.

[0017] Figure 7 The Ti2Nb prepared in Example 3 10 O 29 SEM image of powder.

[0018] Figure 8 The Ti2Nb prepared in Example 3 10 O 29 EDS point analysis spectrum of powder.

[0019] Fig. 9 The Ti2Nb prepared in Example 3 10 O 29 Raman spectrum of powder.

[0020] Fig.10 The Ti2Nb prepared in Example 4 10 O 29 XRD pattern of powder.

[0021] Fig.11 The Ti2Nb prepared in Example 4 10 O 29 SEM image of powder.

[0022] Fig.12 The Ti2Nb prepared in Example 4 10 O 29 EDS point analysis spectrum of powder. DETAILED DESCRIPTION

[0023] The technical solution of the present invention is not limited to the specific embodiments listed below, but also includes any combination of the specific implementation modes.

[0024] Example 1

[0025] In this embodiment, Ti2Nb is prepared 10 O29 The powder process is as follows: Select (Ti 0.2 Nb 0.8 )C micron powder is used as raw material. First, the carbide precursor is placed in a furnace and heated to 800℃ at a heating rate of 5℃ / min in an air atmosphere. The oxidation treatment is carried out at this temperature for 2 hours. After the reaction is completed, the product is naturally cooled to room temperature with the furnace to obtain high-purity Ti2Nb 10 O 29 Powder.

[0026] The (Ti 0.2 Nb 0.8 )C micron powder preparation: TiC, NbC and Co powder are used as raw materials. First, weigh TiC and NbC powders in a molar ratio of 1:4. Then, weigh these carbide powders and Co powder in a mass ratio of 7:3 and mix them evenly. After the mixed powder is pre-pressed into shape through a mold, it is transferred to a furnace. In an argon protective atmosphere, the temperature is heated to 1500°C at a heating rate of 8°C / min and kept warm for 8 hours. After the reaction is completed, the product is allowed to cool naturally to room temperature with the furnace, and (Ti 0.2 Nb 0.8 )C / Co based composite material block. After that, the composite material block is immersed in nitric acid solution to corrode and dissolve the Co alloy matrix. After the corrosion is completed, it is filtered, then repeatedly washed with deionized water and alcohol, and dried to finally obtain (Ti 0.2 Nb 0.8 )C micron powder.

[0027] The prepared TNO powder was subjected to X-ray diffraction phase analysis (XRD). Figure 1 As shown, the obtained XRD diffraction peaks are clear and strong, which is consistent with the monoclinic Ti2Nb 10 O 29 The main diffraction peaks appear at 2θ of about 23.78°, 44.44°, and 47.65°, corresponding to the (011), (700) and (020) crystal planes, respectively, indicating that the sample has good crystallinity. In addition, no diffraction peaks of any impurity phase were observed in the XRD spectrum, confirming that the prepared Ti2Nb 10 O 29 High purity of powder.

[0028] Figure 2 The prepared Ti2Nb 10 O 29 The microstructure of the powder. Figure 2In the SEM image shown in (a), the TNO powder exhibits a tetrahedral morphology, with the side length of the tetrahedral pyramid ranging from 4 to 7.5 μm. The edges of these tetrahedral pyramids are sharp, indicating that the TNO powder has good dispersibility. Figure 2 (b) It further reveals that these micron tetrahedral pyramids are composed of TNO particles with a particle size of 100 to 250 nm. The unique tetrahedral structure and fine particle size of TNO powder help increase the specific surface area of ​​the material and provide more active sites in electrochemical applications. This optimizes its electrochemical performance and makes it an ideal negative electrode material for lithium-ion batteries.

[0029] Figure 3 The prepared Ti2Nb 10 O 29 The EDS point analysis results of the powder. This spectrum reveals the characteristic peaks of four elements: carbon (C), oxygen (O), niobium (Nb) and titanium (Ti). The analysis results show that the atomic percentage of oxygen (O) is the highest, reaching 56.16%. This high ratio indicates the thoroughness of the oxidation process and reflects the high oxidation state of the material. In addition, the molar content ratio of niobium (Nb) to titanium (Ti) is 5.09:1, which is consistent with the Ti2Nb 10 O 29 The stoichiometric ratio of the phase theory is consistent with that of the product, and combined with its XRD spectrum results, it is confirmed that the product is TNO phase. The above results confirm the feasibility and correctness of the synthesis method.

[0030] Example 2

[0031] In this embodiment, Ti2Nb is prepared 10 O 29 The powder process is as follows: Select (Ti 0.2 Nb 0.8 )C micron powder is used as raw material. First, the carbide precursor is placed in a furnace and heated to 900℃ at a heating rate of 5℃ / min in an air atmosphere. The oxidation treatment is carried out at this temperature for 2 hours. After the reaction is completed, the product is naturally cooled to room temperature with the furnace to obtain high-purity Ti2Nb 10 O 29 Powder. (Ti 0.2 Nb 0.8 ) The preparation process of C micron powder precursor is the same as that in Example 1.

[0032] The prepared TNO powder was subjected to X-ray diffraction phase analysis (XRD). Figure 4 As shown, the obtained XRD diffraction peaks are clear and strong, which is consistent with the monoclinic Ti2Nb 10 O 29The main diffraction peaks appear at 2θ of about 23.78°, 44.44°, and 47.65°, corresponding to the (011), (700) and (020) crystal planes, respectively, indicating that the sample has good crystallinity. In addition, no diffraction peaks of any impurity phase were observed in the XRD spectrum, confirming that the prepared Ti2Nb 10 O 29 High purity of powder.

[0033] Figure 5 The prepared Ti2Nb 10 O 29 The microstructure of the powder. Figure 5 In the SEM image shown in (a), the TNO powder exhibits a tetrahedral morphology, and the side length of the tetrahedral pyramid is between 3 and 10 microns. The edges of these tetrahedral pyramids are sharp, indicating that the TNO powder has good dispersibility. Figure 5 (b) It further reveals that these micron tetrahedral pyramids are composed of TNO particles with a particle size of 100 to 200 nm. The unique tetrahedral structure and fine particle size of TNO powder help increase the specific surface area of ​​the material and provide more active sites in electrochemical applications. This optimizes its electrochemical performance and makes it an ideal negative electrode material for lithium-ion batteries.

[0034] Example 3

[0035] In this embodiment, Ti2Nb is prepared 10 O 29 The powder process is as follows: Select (Ti 0.2 Nb 0.8 )C micron powder is used as raw material. First, the carbide precursor is placed in a furnace and heated to 1000°C at a heating rate of 5°C / min in an air atmosphere. The oxidation treatment is carried out at this temperature for 2 hours. After the reaction is completed, the product is naturally cooled to room temperature with the furnace to obtain high-purity Ti2Nb 10 O 29 Powder. (Ti 0.2 Nb 0.8 ) The preparation process of C micron powder precursor is the same as that in Example 1.

[0036] The prepared TNO powder was subjected to X-ray diffraction phase analysis (XRD). Figure 6 As shown, the obtained XRD diffraction peaks are clear and strong, which is consistent with the monoclinic Ti2Nb 10 O 29The main diffraction peaks appear at 2θ of about 23.78°, 24.96°, and 47.65°, corresponding to the (011), (400) and (020) crystal planes, respectively, indicating that the sample has good crystallinity. In addition, no diffraction peaks of any impurity phase were observed in the XRD spectrum, confirming that the prepared Ti2Nb 10 O 29 High purity of powder.

[0037] Figure 7 The prepared Ti2Nb 10 O 29 The microstructure of the powder. Figure 7 In the SEM image shown in (a), the TNO powder exhibits a tetrahedral morphology with a side length of 4 to 7 microns. The edges of these tetrahedral pyramids are sharp, indicating that the TNO powder has good dispersibility. Figure 7 (b) It further reveals that these micron tetrahedral pyramids are composed of TNO particles with a particle size of 100 to 400 nm. The unique tetrahedral structure and fine particle size of TNO powder help increase the specific surface area of ​​the material and provide more active sites in electrochemical applications. This optimizes its electrochemical performance and makes it an ideal negative electrode material for lithium-ion batteries.

[0038] Figure 8 The prepared Ti2Nb 10 O 29 The EDS point analysis results of the powder. This spectrum reveals the characteristic peaks of four elements: carbon (C), oxygen (O), niobium (Nb) and titanium (Ti). The analysis results show that the atomic percentage of oxygen (O) is the highest, reaching 60.44%. This high ratio indicates the thoroughness of the oxidation process and reflects the high oxidation state of the material. In addition, the molar content ratio of niobium (Nb) to titanium (Ti) is 5.03:1, which is consistent with the Ti2Nb 10 O 29 The stoichiometric ratio of the phase theory is consistent with that of the product, and combined with its XRD spectrum results, it is confirmed that the product is TNO phase. The above results confirm the feasibility and correctness of the synthesis method.

[0039] Fig. 9 The Raman spectrum of the prepared TNO powder is shown, and several characteristic peaks are detected, which are located at 112, 132, 164, 267, 348, 539, 645, 891 and 998 cm -1 ; This shows that Ti2Nb 10 O 29 There are many vibration modes in the crystal structure. Among them, the -1 , 132 cm-1 and 164 cm -1 The characteristic peaks reflect the lattice vibrations of Nb and Ti atoms in TNO crystals. -1 and 348 cm -1 The characteristic peaks at 539 cm represent the symmetric and asymmetric bending vibrations of Ti-O and Nb-O bridge oxygen. -1 and 645 cm -1 The characteristic peak of TiO6 represents the metal-oxygen stretching vibration of the TiO6 octahedron, while the peak at 891 cm -1 and 998 cm -1 The characteristic peak is the stretching vibration of Nb-O bond in NbO6 octahedron.

[0040] Example 4

[0041] In this embodiment, Ti2Nb is prepared 10 O 29 The powder process is as follows: Select (Ti 0.2 Nb 0.8 )C micron powder is used as raw material. First, the carbide precursor is placed in a furnace and heated to 1200℃ at a heating rate of 5℃ / min in an air atmosphere. The oxidation treatment is carried out at this temperature for 2 hours. After the reaction is completed, the product is naturally cooled to room temperature with the furnace to obtain high-purity Ti2Nb 10 O 29 Powder. (Ti 0.2 Nb 0.8 ) The preparation process of C micron powder precursor is the same as that in Example 1.

[0042] The prepared TNO powder was subjected to X-ray diffraction phase analysis (XRD). Fig.10 As shown, the obtained XRD diffraction peaks are clear and strong, which is consistent with the monoclinic Ti2Nb 10 O 29 The main diffraction peaks appear at 2θ of about 23.78°, 24.96°, and 26.03°, corresponding to the (011), (400) and (21-1) crystal planes, respectively, indicating that the sample has good crystallinity. In addition, no diffraction peaks of any impurity phase were observed in the XRD spectrum, confirming that the prepared Ti2Nb 10 O 29 High purity of powder.

[0043] Fig.11 The prepared Ti2Nb 10 O 29 The powder has a unique microstructure. Fig.11From the SEM image shown in (a), it can be observed that the TNO powder exhibits a tetrahedral morphology. The surfaces of these micron-sized cones are rough and the edges are jagged. Fig.11 (b) further reveals that the TNO microcones are composed of tightly packed columnar crystals, the length of which is in the range of 1 to 3.5 μm.

[0044] Fig.12 The prepared Ti2Nb 10 O 29 The EDS point analysis results of the powder. This spectrum reveals the characteristic peaks of four elements: carbon (C), oxygen (O), niobium (Nb) and titanium (Ti). The analysis results show that the atomic percentage of oxygen (O) is the highest, reaching 54.27%, indicating the thoroughness of the oxidation process and reflecting the high oxidation state of the material. In addition, the molar content ratio of niobium (Nb) to titanium (Ti) is 4.43:1, which is consistent with the Ti2Nb 10 O 29 The stoichiometric ratio of the phase theory is consistent with that of the product, and combined with its XRD spectrum results, it is confirmed that the product is TNO phase. The above results confirm the feasibility and correctness of the synthesis method.

[0045] Example 5

[0046] In this embodiment, Ti2Nb is prepared 10 O 29 The powder process is as follows: Select (Ti 0.2 Nb 0.8 )C micron powder is used as raw material. First, the carbide precursor is placed in a furnace and heated to 800℃ at a heating rate of 2℃ / min in an air atmosphere. The oxidation treatment is carried out at this temperature for 5 hours. After the reaction is completed, the product is naturally cooled to room temperature with the furnace to obtain high-purity Ti2Nb 10 O 29 Powder. (Ti 0.2 Nb 0.8 ) The preparation process of C micron powder precursor is the same as that in Example 1.

[0047] Example 6

[0048] In this embodiment, Ti2Nb is prepared 10 O 29 The powder process is as follows: Select (Ti 0.2 Nb 0.8 )C micron powder is used as raw material. First, the carbide precursor is placed in a furnace and heated to 1300℃ at a heating rate of 10℃ / min in an air atmosphere. The oxidation treatment is carried out at this temperature for 1 hour. After the reaction is completed, the product is naturally cooled to room temperature with the furnace to obtain high-purity Ti2Nb 10 O 29Powder. (Ti 0.2 Nb 0.8 ) The preparation process of C micron powder precursor is the same as that in Example 1.

Claims

1. A method for preparing Ti2Nb 10 O 29 The method of preparing a powder is characterized by: Selection (Ti 0.2 Nb 0.8 ) C micron powder as raw material; Place it in a furnace and heat it to 800-1300℃ at a heating rate of 2-10℃ / min in an air atmosphere, and keep it at this temperature for 1-5 hours for oxidation treatment. After the reaction is completed, the product is cooled naturally to room temperature in the furnace to obtain Ti2Nb 10 O 29 Powder.

2. The method according to claim 1, wherein said (Ti 0.2 Nb 0.8 The preparation steps of )C micron powder raw material are as follows: (1) weigh TiC and NbC powders in a molar ratio of 1:4; (2) weigh total carbide powder and Co powder in a mass ratio of 7:3 and mix them evenly; (3) pre-press the mixed powder into a mold and transfer it to a furnace. In an argon protective atmosphere, heat the temperature to 1500℃ at a heating rate of 8℃ / min and keep it warm for 8 hours. After the reaction is completed, let the product cool naturally to room temperature in the furnace to obtain (Ti 0.2 Nb 0.8 )C / Co based composite material block; (4) immersing the composite material block in nitric acid solution to dissolve the Co alloy matrix, and obtaining (Ti 0.2 Nb 0.8 )C micron powder.

Citation Information

Patent Citations

  • Method of preparing Bi3TiNbO9 micro-nano piezoelectricity ferro-electricity powder

    CN101100381A

  • Zirconium oxide / titanium oxide / cerium oxide doped rare earth tantalum / niobate RETa / NbO4 ceramic powder and preparation method thereof

    CN109534814A

  • Synthesis method of nitrogen-containing carbon-coated titanium niobate material for lithium battery negative electrode

    CN110911666A

  • In-situ synthesis (TiNb) C reinforced ultrafine grain TiNbMo refractory concentrated alloy-based composite material and preparation method thereof

    CN114438360A

  • Titanium niobium tin oxide electrode material and preparation method thereof

    CN118324184A

Cited By

  • Materials, devices, and methods with compositions for oxide ceramics for extreme environments