Method for preparing lignite-based SiC chopped fiber by using calcium chloride and magnesium chloride as sintering aids
By using calcium chloride and magnesium chloride as sintering additives at low temperatures, high-quality SiC chopped fibers were successfully prepared, solving the generation problems and poor morphology in the existing technology in low temperatures, and realizing the Production of SiC chopped fibers with high content and excellent properties.
Patent Information
- Application Number
- CN202411423816.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The prior art is difficult to generate SiC chopped fibers at low temperatures, and the resulting morphology is poor.
Calcium chloride and magnesium chloride are used as sintering aids, and SiC short-cut fibers are prepared by mixing lignite, silicon source and sintering aids, carbonization and sintering reactions, and then sonication and grinding.
The resulting SiC chopped fibers are about 60nm in diameter, 100nm to 2μm in length, and the mass content reaches 94%. They have excellent electromagnetic wave absorption performance and are suitable for the preparation of high-performance materials.
Smart Images

Figure CN118993740A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing SiC chopped fibers. Background Art
[0002] Lignite is the mineral coal with the lowest degree of coalification. It is a dark brown, dull, low-quality coal with a color between peat and tar coal. SiC is a new type of material with excellent mechanical, electrical and thermal properties. It is widely used in semiconductors, optoelectronic devices, energy and other fields. In industry, there are two main methods for preparing SiC chopped fibers: chemical vapor deposition and physical vapor deposition. SiC chopped fibers have a wide range of applications, especially in the field of electronic devices. Due to its excellent electrical conductivity and thermal stability, they are widely used in microelectronic devices. In addition, SiC chopped fibers can also be used in the preparation of solar cells, catalyst carriers and other fields. However, the generation temperature of existing silicon carbide is generally above 1700°C, and most of the generated morphology is particle morphology, with few nanowires, chopped fibers and other shapes. Summary of the invention
[0003] The present invention aims to solve the problem that the chopped fibers are difficult to generate at low temperature and have poor morphology in the prior art, and provides a method for preparing lignite-based SiC chopped fibers by using calcium chloride and magnesium chloride as sintering aids.
[0004] A method for preparing lignite-based SiC chopped fibers by using calcium chloride and magnesium chloride as sintering aids is completed by the following steps:
[0005] 1. Drying and crushing the lignite to obtain crushed lignite, ball-milling and mixing the crushed lignite, silicon source and sintering aid, and then sieving to obtain mixed powder;
[0006] The sintering aid is a mixture of calcium chloride and magnesium chloride;
[0007] 2. placing the mixed powder in a graphite crucible, and sequentially performing a carbonization reaction and a sintering reaction under an inert atmosphere to obtain a sintered block;
[0008] 3. The sintered block is subjected to ultrasonic treatment, and then crushed and ground, thereby completing the method for preparing lignite-based SiC chopped fibers by using calcium chloride and magnesium chloride as sintering aids.
[0009] The beneficial effects of the present invention are:
[0010] The present invention can reduce the reaction temperature by adding calcium chloride and magnesium chloride as sintering aids, so that the reaction can be more fully reacted below 1600°C, and the content of silicon carbide chopped fibers can be regulated. The mass content of SiC can reach 94%, and the SEM surface morphology has basically no residual raw material morphology. In addition, silicon carbide can be continuously grown along the (111) crystal plane, thereby obtaining more excellent and longer chopped fibers. The diameter of the SiC chopped fibers is about 60nm and the length is 100nm to 2μm. The chopped fibers with a high final content are prepared by a one-step reaction method with a simple process using the cheap raw material of lignite from Zhalainuoer, Inner Mongolia, which can improve the application value of lignite, have important research significance for environmental protection, comply with the national dual-carbon policy, and are conducive to green and sustainable development.
[0011] 1. The present invention uses lignite from Zhalainuoer, Inner Mongolia, which contains an appropriate amount of moisture (16%) and a small amount of ash (10%), and the rest is carbon and organic volatile matter. The ash in the raw material is composed of a small amount of various metal oxides and silicon dioxide, etc. Appropriate metal particles can promote VLS reaction and are conducive to the generation of short-cut fibers.
[0012] 2. The silicon source of the present invention interacts with the carbon component in the lignite through a solid phase reaction to achieve the generation of SiC. The preparation method of the present invention is simple, the one-step reaction process of adding a sintering aid is easy to control, and is suitable for large-scale industrial production. The present invention uses bulk lignite from Zhalainuoer, Inner Mongolia as a raw material, reduces costs, realizes the high-value-added resource utilization of lignite to the greatest extent, and improves my country's lignite comprehensive utilization capacity.
[0013] 3. The chopped fibers generated by the present invention have regular shapes and high content, the mass content of SiC can reach more than 94%, and the diameter is about 60nm, the length ranges from 100nm to 2μm, has a large aspect ratio, is β-SiC, and the crystal phase is 3C phase. It has good electromagnetic wave absorption performance in the range of 2-18GHz. At the optimal thickness of 2.45mm, the minimum reflection loss is -58dB, and the EAB is 5.4GHz. In addition to the electromagnetic wave absorption performance, it is also a high-quality raw material for preparing high-performance silicon carbide ceramics, and can also be used as nanomaterials, fireproof insulation materials and heat storage materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 is the XRD spectrum of the lignite described in step 1 of Example 1;
[0015] Figure 2 This is the XPS spectrum of the lignite described in step 1 of Example 1;
[0016] Figure 3 This is the XRD spectrum of the lignite-based SiC chopped fibers prepared in Example 1;
[0017] Figure 4 This is a scanning electron microscope image of the lignite-based SiC chopped fibers prepared in Example 1;
[0018] Figure 5 This is a transmission electron microscope image of lignite-based SiC chopped fibers prepared in Example 1;
[0019] Figure 6 This is a diagram of the microwave absorption performance of the lignite-based SiC chopped fibers prepared in Example 1. DETAILED DESCRIPTION
[0020] Specific implementation method 1: This implementation method is a method for preparing lignite-based SiC chopped fibers by using calcium chloride and magnesium chloride as sintering aids, which is completed in the following steps:
[0021] 1. Drying and crushing the lignite to obtain crushed lignite, ball-milling and mixing the crushed lignite, silicon source and sintering aid, and then sieving to obtain mixed powder;
[0022] The sintering aid is a mixture of calcium chloride and magnesium chloride;
[0023] 2. placing the mixed powder in a graphite crucible, and sequentially performing a carbonization reaction and a sintering reaction under an inert atmosphere to obtain a sintered block;
[0024] 3. The sintered block is subjected to ultrasonic treatment, and then crushed and ground, thereby completing the method for preparing lignite-based SiC chopped fibers by using calcium chloride and magnesium chloride as sintering aids.
[0025] Principle: Lignite contains fixed carbon, organic carbon (volatile matter) and other substances. Lignite is used as a raw material to introduce a carbon source as a reactant, and then a silicon source is introduced to react under high temperature to achieve the introduction of SiC components. The sintering aid added during the reaction can regulate the morphological growth of silicon carbide, allowing silicon carbide to continue to grow along the (111) crystal plane, thereby obtaining a more excellent microscopic morphology. At the same time, Ar gas is introduced into the high-temperature reaction as an inert atmosphere, and a one-step molding reaction method is used to prepare SiC chopped fibers.
[0026] In the low temperature region (20℃~1100℃), physical adsorption may occur between lignite and the surface of the silicon source, creating conditions for subsequent reactions. As the temperature rises to the medium temperature region (1100℃~1300℃), silicon is adsorbed to the surface of fixed carbon, and organic carbon molecules gradually dissociate to produce carbon atoms. These carbon atoms can be adsorbed on the surface of the silicon source to form a silicon-carbon interface. At this interface, carbon atoms and silicon atoms may react to begin to form silicon carbide (SiC). The reaction at this stage may proceed gradually on the interface, uniformly generating tiny SiC particles. As the temperature further rises to the high temperature region (1300℃~1550℃), the carbonization reaction on the interface may accelerate. Carbon reacts with silicon to form larger SiC crystals. The crystal size and growth process may be affected by factors such as temperature, reaction time, and the crystal structure of the silicon source. In high temperature areas, the carbon in lignite may react with the residual oxygen in the atmosphere to generate carbon monoxide (CO) gas. However, since the oxygen content is too low, it is almost impossible to generate gaseous silicon source (SiO). Therefore, the reaction between lignite and pure silicon powder is mainly a solid-phase reaction mechanism.
[0027] The beneficial effects of this embodiment are:
[0028] This specific embodiment can reduce the reaction temperature by adding calcium chloride and magnesium chloride as sintering aids, so that the reaction can be more fully reacted below 1600°C, and the content of silicon carbide chopped fibers can be regulated. The mass content of SiC can reach 94%, and the SEM surface morphology has basically no residual raw material morphology. In addition, silicon carbide can continue to grow along the (111) crystal plane, thereby obtaining more excellent and longer chopped fibers. The diameter of SiC chopped fibers is about 60nm and the length is 100nm~2μm. The short fibers with a high final content are prepared by a one-step reaction method using a cheap raw material such as lignite from Zhalainuoer, Inner Mongolia, which can improve the application value of lignite, have important research significance for environmental protection, comply with the national dual carbon policy, and are conducive to green and sustainable development.
[0029] 1. This embodiment uses lignite from Zhalainuoer, Inner Mongolia, which contains an appropriate amount of moisture (16%) and a small amount of ash (10%), and the rest is carbon and organic volatile matter. The ash in the raw material is composed of a small amount of various metal oxides and silicon dioxide, etc. Appropriate metal particles can promote VLS reaction and are conducive to the generation of short-cut fibers.
[0030] 2. In this embodiment, the silicon source and the carbon component in the lignite interact through a solid phase reaction to achieve the generation of SiC. The preparation method of this embodiment is simple, and the one-step reaction process of adding a sintering aid is easy to control, which is suitable for large-scale industrial production. This embodiment uses bulk lignite from Zhalainuoer, Inner Mongolia as raw material to reduce costs, maximize the high-value-added resource utilization of lignite, and improve my country's lignite comprehensive utilization capacity.
[0031] 3. The chopped fibers generated in this embodiment have regular shapes and high content, the mass content of SiC can reach more than 94%, and the diameter is about 60nm, the length ranges from 100nm to 2μm, has a large aspect ratio, is β-SiC, and the crystal phase is 3C phase. It has good electromagnetic wave absorption performance in the range of 2-18GHz. At the optimal thickness of 2.45mm, the minimum reflection loss is -58dB, and the EAB is 5.4GHz. In addition to the electromagnetic absorption performance, it is also a high-quality raw material for preparing high-performance silicon carbide ceramics, and can also be used as nanomaterials, fireproof insulation materials and heat storage materials.
[0032] Specific embodiment 2: This embodiment differs from specific embodiment 1 in that: the lignite described in step 1 is lignite from Zhalainuoer, Inner Mongolia; the silicon source described in step 1 is one or a combination of waste silicon powder, pure silicon powder, silicon dioxide and silica. The rest is the same as specific embodiment 1.
[0033] Specific embodiment 3: This embodiment differs from specific embodiment 1 or 2 in that the mass ratio of calcium chloride to magnesium chloride in the sintering aid described in step 1 is (0.9-1.1): 1. The rest is the same as specific embodiment 1 or 2.
[0034] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that: the mass ratio of the crushed lignite to the silicon source in step 1 is (1 to 5):5; the mass ratio of the crushed lignite to the sintering aid in step 1 is 1:(0.01 to 0.03). Others are the same as specific embodiments 1 to 3.
[0035] Specific embodiment 5: This embodiment differs from specific embodiments 1 to 4 in that: the ball milling mixing described in step 1 is specifically carried out at a ball mill speed of 200 r / min to 600 r / min and a ball-to-material ratio of (1.5 to 2):1 for 1 h to 4 h; and the grinding ball material used in the ball milling process is cemented carbide. Other aspects are the same as specific embodiments 1 to 4.
[0036] Specific implementation method 6: This implementation method is different from specific implementation methods 1 to 5 in that: the drying described in step 1 is specifically carried out at a drying temperature of 60°C to 90°C for 1h to 2h; the sieving described in step 1 is specifically carried out through a 60-mesh sieve. The rest is the same as specific implementation methods 1 to 5.
[0037] Specific embodiment 7: This embodiment differs from specific embodiments 1 to 6 in that the inert atmosphere in step 2 is an Ar gas atmosphere, the purity of the Ar gas is ≥ 99.99%, and the flow rate of the Ar gas is 20 mL / min to 100 mL / min. Other aspects are the same as specific embodiments 1 to 6.
[0038] Specific embodiment eight: This embodiment differs from specific embodiments one to seven in that: the carbonization reaction described in step two is specifically carried out at a heating rate of 2°C / min to 5°C / min, the temperature is raised to 600°C to 800°C, and then the temperature is kept at 600°C to 800°C for 2h to 6h. Others are the same as specific embodiments one to seven.
[0039] Specific embodiment 9: This embodiment is different from specific embodiments 1 to 8 in that: the sintering reaction described in step 2 is first heated to 900°C to 1000°C at a rate of 2°C / min to 5°C / min, then heated to 1400°C to 1550°C at a rate of 2°C / min to 2.5°C / min, kept at 1400°C to 1550°C for 1h to 5h, then cooled to 900°C to 1000°C at a rate of 2°C / min to 2.5°C / min, and finally cooled to room temperature at a rate of 2°C / min to 5°C / min. The rest is the same as specific embodiments 1 to 8.
[0040] Specific embodiment 10: This embodiment differs from Specific embodiments 1 to 9 in that the ultrasonic treatment described in step 3 is carried out under the condition of ultrasonic power of 100W to 300W for 0.5h to 1h. The rest is the same as Specific embodiments 1 to 9.
[0041] The following examples are used to verify the beneficial effects of the present invention:
[0042] Embodiment 1:
[0043] A method for preparing lignite-based SiC chopped fibers by using calcium chloride and magnesium chloride as sintering aids is completed by the following steps:
[0044] 1. Dry the lignite for 1 hour at a drying temperature of 80°C, and then crush it to obtain the crushed lignite. At a ball mill speed of 500r / min and a ball-to-material ratio of 2:1, ball-mill the crushed lignite, silicon source and sintering aid for 2 hours, and then pass through a 60-mesh sieve to obtain a mixed powder;
[0045] The sintering aid is a mixture of calcium chloride and magnesium chloride; the mass ratio of calcium chloride to magnesium chloride in the sintering aid is 1:1; the mass ratio of the crushed lignite to the silicon source is 1:1; the mass ratio of the crushed lignite to the sintering aid is 1:0.02;
[0046] 2. placing the mixed powder in a graphite crucible, and sequentially performing carbonization reaction and sintering reaction in a tube furnace under inert atmosphere conditions to obtain a sintered block;
[0047] 3. Under the condition of ultrasonic power of 200W, the sintered block was ultrasonicated for 0.5h, then crushed and ground to obtain lignite-based SiC chopped fibers.
[0048] The lignite described in step 1 is lignite from Zhalainuoer Coal Industry in Inner Mongolia, wherein the mass percentage of moisture in the lignite is 16%, the mass percentage of fixed carbon in the lignite is 38%, the mass percentage of volatile matter in the lignite is 36%, the mass percentage of ash in the lignite is 10%, and the ash is composed of a small amount of various metal oxides and silicon dioxide; the particle size of the lignite described in step 1 is mainly concentrated in the range of 2 μm to 6 μm, and the average particle size is 4 μm;
[0049] The silicon source described in step 1 is waste silicon powder from Inner Mongolia Haite Huacai Co., Ltd., with an average particle size of 1 μm.
[0050] The grinding balls in the ball milling mixing described in step 1 are carbon steel balls.
[0051] The inert atmosphere described in step 2 is an Ar gas atmosphere, the purity of the Ar gas is ≥99.99%, and the flow rate of the Ar gas is 40 mL / min.
[0052] The carbonization reaction described in step 2 is specifically carried out at a heating rate of 2°C / min to 800°C, and then the temperature is kept at 800°C for 4 hours.
[0053] The sintering reaction described in step 2 is specifically to first heat the temperature to 1000°C at a rate of 4°C / min, then heat the temperature to 1500°C at a rate of 2°C / min, keep the temperature at 1500°C for 2 hours, then cool down to 1000°C at a rate of 2°C / min, and finally cool down to room temperature at a rate of 4°C / min.
[0054] In step 2 of this embodiment, a tubular furnace is used. In actual production, the sintering can be expanded by first evacuating the vacuum and then introducing a protective gas before sintering.
[0055] Figure 1 is the XRD spectrum of the lignite described in step 1 of Example 1; Figure 2 This is the XPS spectrum of the lignite described in step 1 of Example 1; it can be seen from the figure that the main elements in lignite are C, O, Si and a small amount of metal peaks. Combining XRD and XPS, it can be obtained that lignite mainly contains graphite phase and amorphous C phase and a small amount of metal oxides and silicon dioxide.
[0056] Figure 3 This is the XRD spectrum of lignite-based SiC chopped fibers prepared in Example 1; as can be seen from the figure, a strong diffraction peak of the 3C phase of β-SiC is produced in the final product, indicating that the product is β-SiC and the crystal phase is 3C phase. After calculation, it is found that the SiC mass content can reach 94%, indicating that the method of this embodiment achieves the introduction of silicon carbide components, and the SiC chopped fibers are successfully prepared by the method of this embodiment.
[0057] Figure 4 This is a scanning electron microscope image of the lignite-based SiC chopped fibers prepared in Example 1. Figure 5 This is a transmission electron microscope image of lignite-based SiC chopped fibers prepared in Example 1. As can be seen from the image, under Ar atmosphere, the reaction products are mostly in the form of chopped fibers with a diameter of about 60nm and a length ranging from 100nm to 2μm, and the SEM surface morphology has basically no raw material morphology left.
[0058] The lignite-based SiC chopped fibers prepared in Example 1 were uniformly mixed with paraffin wax in a ratio of 3:7, and the microwave absorption performance was tested by a coaxial method; Figure 6 This is a graph showing the absorption performance of lignite-based SiC chopped fibers prepared in Example 1. As can be seen from the graph, it has good electromagnetic wave absorption performance in the range of 2-18 GHz, and at the optimal thickness of 2.45 mm, the minimum reflection loss is -58 dB, and the EAB is 5.4 GHz.
Claims
1. A method for preparing lignite-based SiC chopped fibers by using calcium chloride and magnesium chloride as sintering aids, Features It is done in the following steps:
1. Drying and crushing the lignite to obtain crushed lignite, ball-milling and mixing the crushed lignite, silicon source and sintering aid, and then sieving to obtain mixed powder; The sintering aid is a mixture of calcium chloride and magnesium chloride; 2. placing the mixed powder in a graphite crucible, and sequentially performing a carbonization reaction and a sintering reaction under an inert atmosphere to obtain a sintered block; 3. The sintered block is subjected to ultrasonic treatment, and then crushed and ground, thereby completing the method for preparing lignite-based SiC chopped fibers by using calcium chloride and magnesium chloride as sintering aids.
2. A method for preparing lignite-based SiC chopped fibers by using calcium chloride and magnesium chloride as sintering aids according to claim 1, Features The lignite described in step 1 is lignite from Zhalainuoer, Inner Mongolia; the silicon source described in step 1 is one or a combination of several of waste silicon powder, pure silicon powder, silicon dioxide and silica.
3. A method for preparing lignite-based SiC chopped fibers by using calcium chloride and magnesium chloride as sintering aids according to claim 1, Features The mass ratio of calcium chloride to magnesium chloride in the sintering aid described in step 1 is (0.9-1.1):
1.
4. A method for preparing lignite-based SiC chopped fibers by using calcium chloride and magnesium chloride as sintering aids according to claim 1, Features The mass ratio of the crushed lignite to the silicon source in step 1 is (1-5):5; the mass ratio of the crushed lignite to the sintering aid in step 1 is 1:(0.01-0.03).
5. A method for preparing lignite-based SiC chopped fibers by using calcium chloride and magnesium chloride as sintering aids according to claim 1, Features The ball milling mixing described in step 1 is specifically carried out at a ball mill speed of 200r / min to 600r / min and a ball-to-material ratio of (1.5 to 2):1 for 1h to 4h; and the grinding ball material used in the ball milling process is cemented carbide.
6. A method for preparing lignite-based SiC chopped fibers by using calcium chloride and magnesium chloride as sintering aids according to claim 1, Features The drying described in step 1 is specifically drying at a drying temperature of 60° C. to 90° C. for 1 h to 2 h; the screening described in step 1 is specifically screening through a 60-mesh sieve.
7. A method for preparing lignite-based SiC chopped fibers by using calcium chloride and magnesium chloride as sintering aids according to claim 1, Features The inert atmosphere described in step 2 is an Ar gas atmosphere, the purity of the Ar gas is ≥99.99%, and the flow rate of the Ar gas is 20 mL / min to 100 mL / min.
8. A method for preparing lignite-based SiC chopped fibers by using calcium chloride and magnesium chloride as sintering aids according to claim 1, Features The carbonization reaction described in step 2 is specifically carried out at a heating rate of 2°C / min to 5°C / min, heating to 600°C to 800°C, and then keeping the temperature at 600°C to 800°C for 2h to 6h.
9. A method for preparing lignite-based SiC chopped fibers by using calcium chloride and magnesium chloride as sintering aids according to claim 1, Features The sintering reaction described in step 2 is specifically to first heat the temperature to 900°C to 1000°C at a rate of 2°C / min to 5°C / min, then heat the temperature to 1400°C to 1550°C at a rate of 2°C / min to 2.5°C / min, keep the temperature at 1400°C to 1550°C for 1h to 5h, then cool the temperature to 900°C to 1000°C at a rate of 2°C / min to 2.5°C / min, and finally cool the temperature to room temperature at a rate of 2°C / min to 5°C / min.
10. A method for preparing lignite-based SiC chopped fibers by using calcium chloride and magnesium chloride as sintering aids according to claim 1, Features The ultrasonic treatment described in step 3 is specifically carried out at an ultrasonic power of 100W to 300W for 0.5h to 1h.
Citation Information
Patent Citations
Shaped bodies containing short inorganic fibers
CA2047739A1
Method for preparing silicon carbide nano line
CN101386409A
Preparation method of silicon carbide fiber reinforced low-temperature sintered ceramic-based composite material
CN112851384A
Sintering aid modified nano ceramic powder and preparation method thereof
CN113045319A
In-situ generated carbon fiber reinforced silicon carbide ceramic-based composite material and preparation method thereof