Application of acidic resin supported material in preparation of pentaerythritol ester and preparation method of pentaerythritol ester
The preparation process of pentaerythritol esterification reaction catalyzed by acid resin-supported materials is simplified, the complex process of the existing technology is solved, and the efficient pentaerythritol ester synthesis is achieved.
Patent Information
- Application Number
- CN202411061779.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-22
AI Technical Summary
The methods for preparing pentaerythritol esters in the prior art are complex, including multi-step processes and high costs.
The acidic resin-supported material is used as a catalyst to conduct a one-step oxidation esterification reaction through pentaerythritol and C4-C12 fatty aldehyde to simplify the process flow.
Efficient pentaerythritol ester synthesis was achieved, with the conversion rate of aldehyde greater than 70.5% and the esterification rate of pentaerythritol greater than 68%, which greatly simplified the process steps and improved efficiency.
Smart Images

Figure BDA0004978109230000072 
Figure BDA0004978109230000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of organic synthesis, and in particular to application of an acidic resin-supported material in preparing pentaerythritol ester and a method for preparing pentaerythritol ester. Background Art
[0002] Pentaerythritol itself is a polyol organic compound that can be used to produce alkyd resins, synthetic advanced lubricants, plasticizers and surfactants, etc. These applications are widely used in the coating industry, medicine and explosives. Pentaerythritol esters have good thermal stability and lubricity, can maintain stable performance in high temperature environments, and provide good demoulding and flow properties. This property makes pentaerythritol esters suitable for plastic processing, such as extrusion and molding, and can act as effective internal and external lubricants, helping to improve the thermal stability of products. In the rubber industry, pentaerythritol esters are not only used as plasticizers and heat stabilizers, but also play a role in plasticizing and lubricating during rubber plasticizing. It can improve the processing technology of rubber, improve the qualified rate and dimensional stability of rubber products, reduce energy consumption, and improve mixing efficiency. Pentaerythritol ester is an important neopentyl polyol ester. Pentaerythritol ester has many ester groups, and because there is no hydrogen atom at the β position of the quaternary carbon atom, it can form a six-membered ring resonance structure with hydroxyl oxygen, so it has good oxidation stability, thermal stability, low-temperature fluidity and viscosity-temperature performance, etc. It has been widely used in aviation lubricants, automotive lubricants, air compressor oils and fire-resistant hydraulic oils. Due to its unique chemical structure and excellent performance, pentaerythritol ester plays an important role in many industries, including plastic processing, rubber industry, personal care products, and coating and adhesive manufacturing.
[0003] The method for preparing pentaerythritol ester in the prior art mainly includes the following steps: first, starting from the olefin hydroformylation reaction, a shorter-chain olefin reacts with CO and H2 to generate a long-chain fatty aldehyde, which is further oxidized to a long-chain fatty acid, and pentaerythritol and a long-chain fatty acid are used as raw materials, and an esterification reaction occurs in the presence of a catalyst to obtain pentaerythritol ester. The preparation steps are complicated. Summary of the invention
[0004] In view of this, the purpose of the present invention is to provide an application of an acidic resin-supported material in the preparation of pentaerythritol ester and a method for preparing pentaerythritol ester. The present invention provides an application of an acidic resin-supported material in the preparation of pentaerythritol ester, using pentaerythritol and C4-C12 fatty aldehyde as raw materials to directly synthesize pentaerythritol ester in one step, with simple steps.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The invention provides an application of an acidic resin-supported material in preparing pentaerythritol ester. The acidic resin-supported material is used as a catalyst, pentaerythritol and aliphatic aldehyde are used as raw materials to carry out an oxidative esterification reaction to prepare pentaerythritol ester, wherein the aliphatic aldehyde is a C4-C12 aliphatic aldehyde; the acidic resin-supported material comprises an acidic resin carrier and an active metal component supported on the acidic resin carrier.
[0007] Preferably, the active metal component includes Fe 3+ , Cu 2+ 、Co 2+ 、Ni 2+ , Mn 2+ 、Zn 2+ and Ag + One or more of .
[0008] Preferably, the loading amount (supporting amount) of the active metal component in the acidic resin-supported material is 2 to 10 wt %.
[0009] Preferably, the acidic resin carrier includes 732 type cationic resin, polystyrene type acidic resin, macroporous strongly acidic acrylic acid cation exchange resin and 15 One or more of ion exchange resins.
[0010] Preferably, the acidic resin-supported material is prepared by a method comprising the following steps:
[0011] The acidic resin carrier is impregnated into an active metal salt solution and then dried to obtain the acidic resin supported material.
[0012] Preferably, the immersion temperature is 10-80° C. and the immersion time is 1-8 hours.
[0013] Preferably, the drying comprises rotary evaporation and drying in sequence, the temperature of the rotary evaporation is 40-80° C., the temperature of the drying is 60-140° C., and the time is 4-24 hours.
[0014] The present invention also provides a method for preparing pentaerythritol ester, comprising the following steps:
[0015] The pentaerythritol ester is obtained by using an acidic resin-supported material as a catalyst, pentaerythritol and aliphatic aldehyde as raw materials, and carrying out an oxidative esterification reaction in the presence of an oxidation source.
[0016] Preferably, the temperature of the oxidative esterification reaction is 50-200° C. and the time is 5-30 hours.
[0017] Preferably, the molar ratio of the fatty aldehyde to pentaerythritol is 1:1 to 8:1, the oxidation source is oxygen or air, and the space velocity of the oxidation source is 300 to 3000 mL·h-1 ·g -1 .
[0018] The invention provides an application of an acidic resin-supported material in preparing pentaerythritol ester. The acidic resin-supported material is used as a catalyst, pentaerythritol and aliphatic aldehyde are used as raw materials to carry out an oxidative esterification reaction to prepare pentaerythritol ester, wherein the aliphatic aldehyde is a C4-C12 aliphatic aldehyde; the acidic resin-supported material comprises an acidic resin carrier and an active metal component supported on the acidic resin carrier.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The invention uses pentaerythritol and C4-C12 fatty aldehyde as raw materials, directly synthesizes pentaerythritol ester through oxidative esterification reaction in one step, omitting the process of converting fatty aldehyde to fatty acid, and has simple steps.
[0021] Experimental results show that in the oxidative esterification reaction of the present invention, the conversion rate of aldehyde is greater than 70.5%, up to 99.8%, and the esterification rate of pentaerythritol is greater than 68%, up to 97.97%. DETAILED DESCRIPTION
[0022] The invention provides an application of an acidic resin-supported material in preparing pentaerythritol ester. The acidic resin-supported material is used as a catalyst, pentaerythritol and aliphatic aldehyde are used as raw materials to carry out an oxidative esterification reaction to prepare pentaerythritol ester, wherein the aliphatic aldehyde is a C4-C12 aliphatic aldehyde; the acidic resin-supported material comprises an acidic resin carrier and an active metal component supported on the acidic resin carrier.
[0023] In the present invention, the active metal component preferably includes Fe 3+ , Cu 2+ 、Co 2+ 、Ni 2+ , Mn 2+ 、Zn 2+ and Ag + One or more of the above, wherein the active metal component is loaded on the acidic resin carrier in the form of metal ions.
[0024] In the present invention, the loading amount of the active metal component in the acidic resin-supported material is preferably 2 to 10 wt %, more preferably 5 to 8 wt %.
[0025] In the present invention, the acidic resin carrier preferably includes 732 type cationic resin, polystyrene type acidic resin, macroporous strongly acidic acrylic acid cation exchange resin and 15 One or more of ion exchange resins.
[0026] In the present invention, the acidic resin-supported material is preferably prepared by a method comprising the following steps:
[0027] The acidic resin carrier is impregnated into an active metal salt solution and then dried to obtain the acidic resin supported material.
[0028] In the present invention, the immersion temperature is preferably 10 to 80° C., more preferably room temperature, and the immersion time is preferably 1 to 8 hours, more preferably 5 to 6 hours.
[0029] In the present invention, the active metal salt in the active metal salt solution preferably includes one or more of nitrates, sulfates, acetates and chlorides, and the active metal salt more preferably includes one or more of ferric nitrate, ferric sulfate, ferric acetate, ferric chloride, copper nitrate, copper sulfate, copper acetate, copper chloride, cobalt nitrate, cobalt sulfate, cobalt acetate, cobalt chloride, nickel nitrate, nickel sulfate, nickel acetate, nickel chloride, manganese nitrate, manganese sulfate, manganese acetate, manganese chloride, zinc nitrate, zinc sulfate, zinc acetate, zinc chloride, silver nitrate and silver acetate.
[0030] In the present invention, the active metal salt is preferably added to deionized water to fully dissolve the active metal salt to obtain the active metal salt solution.
[0031] In the present invention, the drying preferably includes rotary evaporation and drying in sequence, the rotary evaporation temperature is preferably 40-80°C, the rotary evaporation is used to remove excess water, the drying temperature is preferably 60-140°C, more preferably 100-120°C, the drying time is preferably 4-24h, more preferably 10-12h. In the present invention, the drying is preferably carried out in a blast drying oven.
[0032] The present invention also provides a method for preparing pentaerythritol ester, comprising the following steps:
[0033] The pentaerythritol ester is obtained by using an acidic resin-supported material as a catalyst, pentaerythritol and aliphatic aldehyde as raw materials, and carrying out an oxidative esterification reaction in the presence of an oxidation source.
[0034] In the present invention, the temperature of the oxidative esterification reaction is preferably 50 to 200° C., more preferably 80 to 130° C., more preferably 100° C., and the time is preferably 5 to 30 h, more preferably 12 to 24 h.
[0035] In the present invention, the molar ratio of the fatty aldehyde to pentaerythritol is preferably 1:1 to 8:1, more preferably 4:1, and the space velocity of the oxidation source is preferably 300 to 3000 mL·h -1 ·g -1 , more preferably 1000 to 1200 mL·h -1 ·g -1, the oxidation source is preferably oxygen or air.
[0036] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] Example 1
[0038] Weigh 1.931 g Co S Dissolve O4·7H2O in 20mL of deionized water, wait until it is fully dissolved, weigh 5g 15 ion exchange resin was added to the metal solution and stirred for 5 hours, then the excess water was evaporated at 80°C, and the obtained solid particles were kept in a 120°C forced air drying oven for 12 hours, cooled to room temperature, and taken out. 15 ion exchange resin catalyst, in which the content of Co ions is 5wt%, recorded as CAT-1.
[0039] Example 2
[0040] Weigh 0.687g MnSO4 and dissolve it in 20mL deionized water. After it is fully dissolved, weigh 5g 15 ion exchange resin was added to the metal solution and stirred for 5 hours, then the excess water was evaporated at 80°C, and the obtained solid particles were kept in a 120°C forced air drying oven for 12 hours, cooled to room temperature, and taken out. 15 ion exchange resin catalyst, in which the content of Mn ions is 5wt%, recorded as CAT-2.
[0041] Example 3
[0042] Weigh 1.802g Fe(NO3)3·9H2O and dissolve it in 20mL deionized water. After it is fully dissolved, weigh 5g 15 ion exchange resin was added to the metal solution and stirred for 5 hours, then the excess water was evaporated at 80°C, and the obtained solid particles were kept in a 120°C forced air drying oven for 12 hours, cooled to room temperature, and taken out. 15 ion exchange resin catalyst, in which the content of Fe ions is 5wt%, and is recorded as CAT-3.
[0043] Example 4
[0044] Weigh 0.391g AgNO3 and dissolve it in 20mL deionized water. After it is fully dissolved, weigh 5g 15 ion exchange resin was added to the metal solution and stirred for 5 hours, then the excess water was evaporated at 80°C, and the obtained solid particles were kept in a 120°C forced air drying oven for 12 hours, cooled to room temperature, and taken out. 15 ion exchange resin catalyst, in which the content of Ag ions is 5wt%, recorded as CAT-4.
[0045] Example 5
[0046] Weigh 0.596g CoSO4·7H2O and 0.343g MnSO4 and dissolve them in 20mL deionized water. After they are fully dissolved, weigh 5g 15 ion exchange resin was added to the metal solution and stirred for 5 hours, then the excess water was evaporated at 80°C, and the obtained solid particles were kept in a 120°C forced air drying oven for 12 hours, cooled to room temperature, and taken out. 15 ion exchange resin catalyst, in which the total content of Co ions and Mn ions is 5wt%, recorded as CAT-5.
[0047] Example 6
[0048] Weigh 0.596g CoSO4·7H2O and 0.901g Fe(NO3)3·9H2O and dissolve them in 20mL deionized water. After they are fully dissolved, weigh 5g 15 ion exchange resin was added to the metal solution and stirred for 5 hours, then the excess water was evaporated at 80°C, and the obtained solid particles were kept in a 120°C forced air drying oven for 12 hours, cooled to room temperature, and taken out. 15 ion exchange resin catalyst, in which the total content of Co ions and Fe ions is 5%, is recorded as CAT-6.
[0049] Example 7
[0050] Weigh 0.596g CoSO4·7H2O and 0.1955g AgNO3 and dissolve them in 20mL deionized water. After they are fully dissolved, weigh 5g 15 ion exchange resin was added to the metal solution and stirred for 5 hours, then the excess water was evaporated at 80°C, and the obtained solid particles were kept in a 120°C forced air drying oven for 12 hours, cooled to room temperature, and taken out. 15 ion exchange resin catalyst, in which the total content of Co ions and Ag ions is 5wt%, and is recorded as CAT-7.
[0051] Example 8
[0052] Weigh 0.901g Fe(NO3)3·9H2O and 0.434g MnSO4 and dissolve them in 20mL deionized water. After they are fully dissolved, weigh 5g 15 ion exchange resin was added to the metal solution and stirred for 5 hours, then the excess water was evaporated at 80°C, and the obtained solid particles were kept in a 120°C forced air drying oven for 12 hours, cooled to room temperature, and taken out. 15 ion exchange resin catalyst, in which the total content of Fe ions and Mn ions is 5wt%, recorded as CAT-8.
[0053] Example 9
[0054] Weigh 0.901g Fe(NO3)3·9H2O and 0.1955g AgNO3 and dissolve them in 20mL deionized water. After they are fully dissolved, weigh 5g 15 ion exchange resin was added to the metal solution and stirred for 5 hours, then the excess water was evaporated at 80°C, and the obtained solid particles were kept in a 120°C forced air drying oven for 12 hours, cooled to room temperature, and taken out. 15 ion exchange resin catalyst, in which the total content of Fe ions and Ag ions is 5wt%, recorded as CAT-9.
[0055] Example 10
[0056] Weigh 0.434g MnSO4 and 0.1955g AgNO3 and dissolve them in 20mL deionized water. After they are fully dissolved, weigh 5g 15 ion exchange resin was added to the metal solution and stirred for 5 hours, then the excess water was evaporated at 80°C, and the obtained solid particles were kept in a 120°C forced air drying oven for 12 hours, cooled to room temperature, and taken out. 15 ion exchange resin catalyst, in which the total content of Mn ions and Ag ions is 5wt%, recorded as CAT-10.
[0057] Embodiment 11
[0058] Weigh 0.7724g Co S Dissolve O4·7H2O in 20mL of deionized water, wait until it is fully dissolved, weigh 5g 15 ion exchange resin was added to the metal solution and stirred for 5 hours, then the excess water was evaporated at 80°C, and the obtained solid particles were kept in a 120°C forced air drying oven for 12 hours, cooled to room temperature, and taken out. 15 ion exchange resin catalyst, in which the content of Co ions is 2wt%, recorded as CAT-11.
[0059] Example 12
[0060] Weigh 3.862g Co S Dissolve O4·7H2O in 20mL of deionized water, wait until it is fully dissolved, weigh 5g 15 ion exchange resin was added to the metal solution and stirred for 5 hours, then the excess water was evaporated at 80°C, and the obtained solid particles were kept in a 120°C forced air drying oven for 12 hours, cooled to room temperature, and taken out. 15 ion exchange resin catalyst, in which the content of Co ions is 10wt%, recorded as CAT-12.
[0061] Embodiment 13
[0062] Weigh 0.2748g MnSO4 and dissolve it in 20mL deionized water. After it is fully dissolved, weigh 5g 15 ion exchange resin was added to the metal solution and stirred for 5 hours, then the excess water was evaporated at 80°C, and the obtained solid particles were kept in a 120°C forced air drying oven for 12 hours, cooled to room temperature, and taken out. 15 ion exchange resin catalyst, in which the content of Mn ions is 2wt%, recorded as CAT-13.
[0063] Embodiment 14
[0064] Weigh 1.374g MnSO4 and dissolve it in 20mL deionized water. After it is fully dissolved, weigh 5g 15 ion exchange resin was added to the metal solution and stirred for 5 hours, then the excess water was evaporated at 80°C, and the obtained solid particles were kept in a 120°C forced air drying oven for 12 hours, cooled to room temperature, and taken out. 15 ion exchange resin catalyst, in which the content of Mn ions is 10wt%, recorded as CAT-14.
[0065] Application Examples 1 to 14
[0066] 1 g of the supported catalyst material prepared in Examples 1 to 14 was weighed respectively, and pentaerythritol (50 mmol) and 3,5,5-trimethylhexanal were used as raw materials, and the molar ratio of pentaerythritol to 3,5,5-trimethylhexanal was 1:4. The mixture was added into a 250 mL three-necked flask, and placed in a metal sand bath with magnetic stirring. The mixture was stirred at an oxygen space velocity of 1200 mL·h -1 ·g -1 Under the conditions, the temperature was raised to the reaction temperature and maintained for a certain time, the reaction was stopped and cooled to room temperature, and the reaction products were analyzed. See Table 1.
[0067] Application Example 15
[0068] 1 g of the supported catalyst material prepared in Example 1 was weighed, pentaerythritol (50 mmol) and n-valeraldehyde were used as raw materials, and the molar ratio of pentaerythritol to n-valeraldehyde was 1:4. The mixture was added into a 250 mL three-necked flask, and placed in a metal sand bath with magnetic stirring. The mixture was stirred at an oxygen space velocity of 1200 mL·h-1 ·g -1 Under the conditions, the temperature was raised to the reaction temperature and maintained for a certain time, the reaction was stopped and cooled to room temperature, and the reaction products were analyzed. See Table 1.
[0069] Application Example 16
[0070] 1 g of the supported catalyst prepared in Example 1 was weighed, and pentaerythritol (50 mmol) and n-heptanal were added into a 250 mL three-necked flask with a molar ratio of pentaerythritol to n-heptanal of 1:4 as raw materials. The flask was placed in a metal sand bath with magnetic stirring and heated at an oxygen space velocity of 1200 mL h -1 ·g -1 Under the conditions, the temperature was raised to the reaction temperature and maintained for a certain time, the reaction was stopped and cooled to room temperature, and the reaction products were analyzed. See Table 1.
[0071] The reaction product is diluted with an organic solvent, and the solid catalyst in the reaction product is filtered out using column chromatography silica gel. The acid value of unreacted fatty acids in the reaction product remaining after filtration is titrated with KOH solution to calculate the esterification rate.
[0072] As can be seen from Table 1, the present invention can obtain pentaerythritol ester by catalyzing the oxidative esterification reaction with an acidic resin-supported catalyst. In the oxidative esterification reaction provided by the present invention, the conversion rate of aldehyde is greater than 70.5%, up to 99.8%, and the esterification rate of pentaerythritol is greater than 68%, up to 97.97%.
[0073] Table 1 Conditions and test results of application examples 1 to 16
[0074]
[0075]
[0076] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.
Claims
1. An application of an acidic resin-supported material in the preparation of pentaerythritol ester, wherein the acidic resin-supported material is used as a catalyst, pentaerythritol and aliphatic aldehyde are used as raw materials for an oxidative esterification reaction to prepare pentaerythritol ester, wherein the aliphatic aldehyde is a C4-C12 aliphatic aldehyde; the acidic resin-supported material comprises an acidic resin carrier and an active metal component supported on the acidic resin carrier.
2. The use according to claim 1, It is characterized in that The active metal component includes Fe 3+ , Cu 2+ 、Co 2+ 、Ni 2 + , Mn 2+ 、Zn 2+ and Ag + One or more of .
3. The use according to claim 1 or 2, It is characterized in that The loading amount of the active metal component in the acidic resin-supported material is 2-10 wt %.
4. The use according to claim 1, It is characterized in that The acid resin carrier includes 732 type cationic resin, polystyrene type acidic resin, macroporous strong acid acrylic acid cation exchange resin and 15 One or more of ion exchange resins.
5. The use according to claim 1, It is characterized in that The acidic resin supported material is prepared by a method comprising the following steps: The acidic resin carrier is impregnated into an active metal salt solution and then dried to obtain the acidic resin supported material.
6. The use according to claim 5, It is characterized in that The immersion temperature is 10-80° C. and the immersion time is 1-8 hours.
7. The use according to claim 5, It is characterized in that The drying comprises rotary evaporation and drying in sequence, wherein the temperature of the rotary evaporation is 40 to 80° C., the temperature of the drying is 60 to 140° C., and the time is 4 to 24 hours.
8. A method for preparing pentaerythritol ester, It is characterized in that The following steps are involved: The pentaerythritol ester is obtained by using an acidic resin-supported material as a catalyst, pentaerythritol and aliphatic aldehyde as raw materials, and carrying out an oxidative esterification reaction in the presence of an oxidation source.
9. The preparation method according to claim 8, It is characterized in that The temperature of the oxidative esterification reaction is 50-200° C. and the time is 5-30 hours.
10. The preparation method according to claim 8, It is characterized in that The molar ratio of the fatty aldehyde to pentaerythritol is 1:1 to 8:1, the oxidation source is oxygen or air, and the space velocity of the oxidation source is 300 to 3000 mL·h -1 ·g -1 .