Preparation method and application of mono-benzyl amino caprolactam and functional nylon-6
By loading active components such as Pt and Pd onto a silicon-modified alumina support, the problems of low catalytic efficiency and environmental pollution in the preparation of monobenzylaminocaprolactam have been solved, realizing efficient and green production and the preparation of functional nylon-6 materials.
Patent Information
- Application Number
- CN202310573386.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-05-19
AI Technical Summary
Existing processes for preparing monobenzylaminocaprolactam suffer from problems such as low catalytic efficiency, harsh reaction conditions, low safety, environmental pollution, poor catalyst stability, and high cost.
By using a supported catalyst, active components such as Pt and Pd are loaded onto a silica-modified alumina support, and combined with specific reaction conditions and solvents, monobenzylaminocaprolactam is prepared. The density of the Brønsted acid on the catalyst support and the dispersion of the active components are optimized to improve the conversion rate of raw materials and the selectivity of the target product.
It improved the raw material conversion rate and target product selectivity, simplified the process flow, realized green production, and produced functional nylon-6 materials with antibacterial, wear-resistant, and impact-resistant properties.
Smart Images

Figure CN118994009A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of organic synthesis, and in particular to a preparation method of monobenzylaminocaprolactam and application thereof, and functional nylon-6. Background Art
[0002] Caprolactam is a monomer of nylon-6, fiber and engineering plastics. It is widely used in textile, automobile, electronics and medical and health industries, and is an important basic organic chemical. At present, my country is the world's largest producer of caprolactam, with an annual output of 5 million tons. However, the rapid growth of caprolactam production capacity has also brought about problems such as oversupply and fierce market competition. It is necessary to actively expand and develop new application areas of caprolactam. Among them, the market demand for nylon materials with antibacterial, wear-resistant and impact-resistant properties is large, but due to problems in material performance and manufacturing costs, these functional materials are mostly in the laboratory research and development stage. Starting from caprolactam or its derivatives, functional modification is carried out on them to obtain functional caprolactam monomers with special structures and properties, which can realize the preparation of functional nylon materials such as intrinsic antibacterial and wear-resistant from the level of polymerized monomers.
[0003] CN102093292A discloses a method for preparing DL-α-aminocaprolactam, which comprises: dissolving α-halogenated caprolactam and benzylamine in an organic solvent, adding a base, and controlling the reaction temperature to react to generate N-benzyl-DL-α-aminocaprolactam; adding the N-benzyl-DL-α-aminocaprolactam generated by the above reaction into a reflux solvent, then adding a catalyst and a hydrogen supply reagent, reflux reaction, and post-processing to obtain the target product DL-α-aminocaprolactam.
[0004] Tao Youhua's team from the Changchun Institute of Applied Chemistry (Chen J., et al, Macromolecules, 2017, 50, 9128-9134) used aminocaprolactam and benzaldehyde as reactants and hydrogenated them in methanol over sodium borohydride to obtain functional caprolactam derived from monobenzyl and disenzyl groups.
[0005] Parker et al. (Parker MF, et al., Bioorganic & Medicinal Chemistry Letters, 2007, 17, 5790-5795) from the R&D department of Bristol-Myers Squibb (BMS) in the United States also used aminocaprolactam and benzaldehyde as reactants and hydrogenated them in methanol with sodium cyanoborohydride and zinc chloride to obtain monobenzyl-derived functional caprolactam.
[0006] Although the above research has promoted the development of the synthetic route of monobenzyl-derived functional caprolactam to a certain extent, there are the following problems: 1) Halides are highly toxic and have poor chemical stability, which will cause serious pollution to the environment; 2) The efficiency of organic reactions is low, and the reaction system is not green, which puts great pressure on the environmental protection and is not conducive to the large-scale production of the target product; 3) Borohydrides are expensive and have poor stability, and are not ideal hydrogenation reagents.
[0007] Therefore, the development of efficient and low-cost catalysts and supporting catalytic reaction systems is of great significance to promoting the development of functional caprolactam monomer catalytic synthesis systems and the production, application and promotion of monomers. Summary of the invention
[0008] The purpose of the invention is to overcome the problems of low catalytic efficiency, harsh reaction conditions, low safety, environmental pollution, poor catalyst stability, high cost, etc. in the existing process of monobenzylaminocaprolactam, and to provide a preparation method of monobenzylaminocaprolactam and application thereof, and a functional nylon-6. The preparation method not only effectively improves the raw material conversion rate and the target product selectivity, but also simplifies the process flow to achieve green production.
[0009] In order to achieve the above object, the first aspect of the present invention provides a method for preparing monobenzylaminocaprolactam, which comprises: contacting and reacting aminocaprolactam and / or its derivatives with benzaldehyde in the presence of a catalyst and a solvent to obtain monobenzylaminocaprolactam.
[0010] Preferably, the reaction conditions include: temperature of 30-150° C.; time of 0.5-16 h; and hydrogen pressure of 0.1-10 MPa.
[0011] Preferably, the mass ratio of the aminocaprolactam and / or its derivatives to benzaldehyde is 1:0.2-2, preferably 1:0.4-1.2.
[0012] Preferably, the mass ratio of the aminocaprolactam and / or its derivatives to the catalyst is 1:0.1-10, preferably 1:0.5-2.
[0013] Preferably, the catalyst is selected from supported catalysts, which include a carrier and an active component supported on the carrier.
[0014] Preferably, the carrier is selected from silicon-modified alumina with a Br acid density of 0-0.5 μmol / g, and the silicon-modified alumina comprises silicon and alumina; wherein the silicon-aluminum ratio of the silicon-modified alumina is less than 1, the silicon is connected to the surface of the alumina through Si-O-Al chemical bonds, and adjacent silicon on the surface of the alumina is connected through Si-O-Si chemical bonds.
[0015] Preferably, the specific surface area of the silicon-modified alumina is 100-220 m 2 / g, preferably 120-200m 2 / g; average pore size is 10-30nm, preferably 15-25nm; wear index is 1-20%, preferably 1-15%; crushing strength is 50-150N / cm, preferably 70-130N / cm.
[0016] Preferably, the active component is selected from at least one of Pt, Pd, Rh, Ir, Ru and Ni, preferably Pt and / or Pd.
[0017] Preferably, the dispersion degree of the active ingredient is ≥20%, preferably 20-80%.
[0018] The second aspect of the present invention provides a use of monobenzylaminocaprolactam prepared by the preparation method provided in the first aspect as a polymerization monomer in the preparation of functional nylon-6.
[0019] The third aspect of the present invention provides a functional nylon-6, wherein the functional nylon-6 contains the monobenzylaminocaprolactam prepared by the preparation method provided by the first aspect.
[0020] Through the above technical scheme, the preparation method of monobenzylaminocaprolactam provided by the present invention uses aminocaprolactam and / or its derivatives and benzaldehyde as raw materials, and then combines a catalyst and a solvent, which can effectively improve the raw material conversion rate and the selectivity of the target product, especially by regulating the carrier and active components of the catalyst, limiting the B acid density of the specific carrier and the dispersion of the specific active components, as well as the mass ratio of each material and the reaction conditions, so as to further improve the catalytic efficiency; at the same time, the catalyst used in the preparation method has the characteristics of stable structure and low cost, and the preparation method also has the advantages of simplified process flow, simple operation, environmental friendliness, and convenience for industrial production.
[0021] At the same time, the monobenzylaminocaprolactam prepared by the preparation method provided by the present invention is used as a polymerization monomer to prepare functional nylon-6 with antibacterial, wear-resistant, impact-resistant, flame-retardant, luminescent and other properties, thereby improving the comprehensive performance of functional nylon-6. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a synthetic route of monobenzylaminocaprolactam provided by the present invention;
[0023] Figure 2 This is the TEM characterization image of the catalyst Pd / AS-1 prepared in Preparation Example 1.
[0024] Figure 3The infrared characterization spectra of pyridine in the catalyst carriers prepared in Preparation Examples 1 and 9-10 are shown in FIG. 1 , wherein the wave number is 1540 cm -1 The absorption peak at indicates the B acid site on the support surface.
[0025] Figure 4 (a) is the transmission infrared spectrum of the carrier AS-1 obtained in Preparation Example 1, Figure 4 (b) Transmission infrared spectrum of the carrier Ac-9 obtained in Preparation Example 9, wherein the wave number is 1066 cm -1 and 1160cm -1 The signal peaks at are the vibration absorption peaks of Si-O-Si and Si-O-Al bonds respectively;
[0026] Figure 5 This is a glass transition temperature curve of functional nylon-6 with different doping amounts prepared in Test Example 1. DETAILED DESCRIPTION
[0027] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0028] In the present invention, unless otherwise specified, "first", "second" and "third" do not indicate a sequence or limit the materials or steps, but are only used to distinguish that they are not the same materials or steps. For example, in "first mixing", "second mixing" and "third mixing", "first", "second" and "third" are only used to indicate that they are not the same mixing.
[0029] The first aspect of the present invention provides a method for preparing monobenzylaminocaprolactam, which comprises: contacting and reacting aminocaprolactam and / or its derivatives with benzaldehyde in the presence of a catalyst and a solvent to obtain monobenzylaminocaprolactam.
[0030] In some embodiments of the present invention, Figure 1 As shown, α-amino-ε-caprolactam and benzaldehyde are contacted and reacted in the presence of a catalyst and a solvent to obtain monobenzyl-α-amino-ε-caprolactam.
[0031] In some embodiments of the present invention, preferably, the reaction conditions include: temperature of 30-150°C; time of 0.5-16h; hydrogen pressure of 0.1-10MPa; further preferably, the reaction conditions include: temperature of 60-120°C; time of 1-3h; hydrogen pressure of 0.5-5MPa. In the present invention, unless otherwise specified, pressure refers to gauge pressure.
[0032] In some embodiments of the present invention, preferably, the mass ratio of aminocaprolactam and / or its derivatives to benzaldehyde is 1:0.2-2, for example, 1:0.2, 1:0.4, 1:0.5, 1:0.8, 1:1, 1:1.2, 1:2, and any value in the range of any two values, preferably 1:0.4-1.2. The preferred mass ratio range is more conducive to improving the selectivity of the target product, thereby improving the yield of the target product.
[0033] In some embodiments of the present invention, preferably, the mass ratio of the aminocaprolactam and / or its derivatives to the catalyst is 1:0.1-10, for example, 1:0.1, 1:0.5, 1:1, 1:1.5, 1:2, 1:5, 1:10, and any value in the range of any two values, preferably 1:0.5-2. The mass ratio meeting the above range is more conducive to improving the conversion rate of the raw materials, thereby improving the yield of the target product.
[0034] In some embodiments of the present invention, preferably, the mass ratio of the aminocaprolactam and / or its derivatives to the solvent is 1:20-200, for example, 1:20, 1:40, 1:50, 1:80, 1:100, 1:150, 1:200, and any value in the range consisting of any two values, preferably 1:40-100.
[0035] In the present invention, unless otherwise specified, the aminocaprolactam and / or its derivatives are selected from aminocaprolactam and / or aminocaprolactam derivatives.
[0036] In some embodiments of the present invention, preferably, the aminocaprolactam and / or its derivatives are selected from aminocaprolactam and / or aminocaprolactam salts. In the present invention, the aminocaprolactam salts include but are not limited to at least one of hydrochloride, sulfate and nitrate.
[0037] In some embodiments of the present invention, further preferably, the aminocaprolactam and / or its derivatives are selected from at least one of DL-α-amino-ε-caprolactam, DL-α-amino-ε-caprolactam hydrochloride, DL-α-amino-ε-caprolactam sulfate and DL-α-amino-ε-caprolactam nitrate.
[0038] In the present invention, the type of the solvent has a wide selection range. Preferably, the solvent is selected from organic solvents, preferably at least one selected from organic alcohols, heteroatom-containing cycloalkanes, heteroatom-containing alkanes, esters and aromatic hydrocarbons.
[0039] In a specific embodiment of the present invention, preferably, when the solvent is selected from organic alcohols, the organic alcohol is selected from C1-C5 organic alcohols, including but not limited to methanol, ethanol, 1-pentanol and 1-hexanol.
[0040] In a specific embodiment of the present invention, preferably, when the solvent is selected from heteroatom-containing cycloalkanes, the heteroatom-containing cycloalkanes include but are not limited to 1,4-dioxane, tetrahydrofuran and the like.
[0041] In a specific embodiment of the present invention, preferably, when the solvent is selected from heteroatom-containing alkanes, the heteroatom-containing alkanes include but are not limited to dimethyl sulfoxide, DMF and the like.
[0042] In a specific embodiment of the present invention, preferably, when the solvent is selected from esters, the esters include but are not limited to ethyl acetate, propyl acetate and the like.
[0043] In a specific embodiment of the present invention, preferably, when the solvent is selected from aromatic hydrocarbons, the aromatic hydrocarbons include but are not limited to benzene, toluene and the like.
[0044] In the present invention, the type of the catalyst is a conventional catalyst in the art, that is, a shaped catalyst. Preferably, the catalyst is a supported metal catalyst, and the supported catalyst comprises a carrier and an active component supported on the carrier; further preferably, based on the total weight of the catalyst, the content of the carrier is 90-99.9wt%, preferably 95-99.5wt%; the content of the active component is 0.1-10wt%, preferably 0.5-5wt%.
[0045] In some embodiments of the present invention, preferably, the carrier is selected from at least one of activated carbon, oxides, molecular sieves and modified oxides, preferably selected from oxides and / or modified oxides. The oxides include but are not limited to SiO2, Al2O3, TiO2, ZrO2 and CeO2, etc.; the molecular sieves include but are not limited to HY molecular sieves, HZSM-5 molecular sieves, etc.; the modified oxides include but are not limited to silicon-modified alumina.
[0046] In some embodiments of the present invention, preferably, the active component is selected from at least one of Pt, Pd, Rh, Ir, Ru and Ni, preferably Pt and / or Pd.
[0047] In some embodiments of the present invention, preferably, the dispersion degree of the active ingredient is ≥20%, for example, 20%, 30%, 40%, 50%, 60%, 80%, and any value in the range consisting of any two values, preferably 20-80%.
[0048] In some embodiments of the present invention, preferably, the support is selected from modified oxides, preferably from silicon-modified oxides, and more preferably from silicon-modified alumina having a B acid density of ≤2 μmol / g.
[0049] In some embodiments of the present invention, preferably, the silicon-modified alumina comprises silicon and alumina; wherein the silicon-to-alumina ratio of the silicon-modified alumina is less than 1, the silicon is connected to the surface of the alumina via Si-O-Al chemical bonds, and adjacent silicon on the surface of the alumina is connected via Si-O-Si chemical bonds.
[0050] In the present invention, unless otherwise specified, the silicon in the silicon-modified alumina is connected to the surface of the alumina through a Si-O-Al chemical bond, which means that Si and Al in the alumina share a portion of O, thereby making SiO x The silicon in the present form is anchored on the surface of the aluminum oxide.
[0051] The inventors of the present invention have found that the surface of alumina has complex acid sites, and the acid sites of different types and strengths have greatly limited the application of alumina in the field of fine chemicals. Therefore, silicon is loaded on the surface of alumina, and silicon is limited to be connected to the surface of alumina through Si-O-Al chemical bonds, and adjacent silicon on the surface of alumina is limited to be connected through Si-O-Si chemical bonds. Under the premise of ensuring that the silicon-modified alumina has a low wear index, high crushing strength, high specific surface area and low average pore size, the acid sites on the surface of alumina can be effectively masked, and the B acid density on the surface of the silicon-modified alumina can be regulated, so that the B acid density of the silicon-modified alumina is ≤2μmol / g.
[0052] In the present invention, unless otherwise specified, B acid density refers to Acid density.
[0053] In the present invention, the B acid density parameter is calculated based on the amount of pyridine desorbed by temperature increase; B acid density = the amount of acid of silicon-modified alumina measured by infrared spectrum of pyridine (in μmol) / the mass of silicon-modified alumina (in g).
[0054] In some embodiments of the present invention, preferably, the B acid density of the silicon-modified alumina is 0-2 μmol / g, for example, 0 μmol / g, 0.1 μmol / g, 0.2 μmol / g, 0.3 μmol / g, 0.5 μmol / g, 0.8 μmol / g, 1 μmol / g, 1.4 μmol / g, 1.5 μmol / g, 2 μmol / g, and any value in the range consisting of any two values, preferably 0-1.4 μmol / g, more preferably 0-0.5 μmol / g.
[0055] In some embodiments of the present invention, based on the total weight of the silicon-modified alumina, the content of the alumina is 50-90wt%, preferably 70-80wt%; x The silicon content is 10-50wt%, preferably 20-30wt%, wherein 1≤x≤2. The preferred conditions are more conducive to reducing the B acid density of silicon-modified alumina.
[0056] In the present invention, unless otherwise specified, the silicon-modified alumina contains no other impurities except silicon and alumina, that is, the sum of the contents of silicon and alumina in the silicon-modified alumina is 100 wt%.
[0057] In some embodiments of the present invention, preferably, the morphology of the silicon-modified alumina is selected from spherical and strip-shaped, wherein the spherical shape includes but is not limited to micro-spherical and small spherical shapes. In the present invention, the macroscopic morphology of the silicon-modified alumina is measured using a scanning electron microscope.
[0058] In some embodiments of the present invention, preferably, the alumina is selected from γ-alumina. The preferred conditions are more conducive to improving the activity of the modified alumina.
[0059] In some embodiments of the present invention, preferably, the specific surface area of the silicon-modified alumina is 100-220 m 2 / g, preferably 120-200m 2 / g; average pore size is 10-30nm, preferably 15-25nm; wear index is 1-20%, preferably 1-15%; crushing strength is 50-150N / cm, preferably 70-130N / cm.
[0060] In the present invention, unless otherwise specified, the specific surface area parameter is measured using a fully automatic isothermal adsorption instrument; the average pore size parameter is measured using a fully automatic isothermal adsorption instrument in combination with the BJH model; the wear index parameter is measured using a wear index analyzer; and the crushing strength parameter is measured using a particle strength tester.
[0061] In the present invention, the preparation method of the silicon-modified alumina has a wide range of selection, as long as the silicon-modified alumina meets the above parameter limitations. Preferably, the silicon-modified alumina is prepared by the following method:
[0062] (1) performing a first mixing of an aluminum source, an acidic compound, and water to obtain a first mixture;
[0063] (2) subjecting the first mixture to molding, first drying and first calcination in sequence to obtain molded alumina;
[0064] (3) dissolving the shaped alumina in water, first adding an alkaline compound to adjust the pH to 7-12, and then adding a silicon source for a second mixing to obtain a second mixture;
[0065] (4) subjecting the second mixture to solid-liquid separation, and subjecting the obtained silicon-modified alumina precursor to a second drying and a second calcination in sequence to obtain the silicon-modified alumina.
[0066] In some embodiments of the present invention, preferably, in step (1), the content of the aluminum source in the first mixture is 0.01-10wt%, preferably 0.05-5wt%; the content of the acidic compound is 0.01-3wt%, preferably 0.05-1wt%. In the present invention, the feed amount / dosage ratio of the aluminum source, the acidic compound and water meets the above definition.
[0067] In the present invention, the type of the aluminum source has a wide range of choices. Preferably, the aluminum source is a soluble aluminum salt, including but not limited to γ-alumina, aluminum oxide hydroxide, pseudo-boehmite, aluminum chloride, aluminum nitrate, etc. When the aluminum source is selected from γ-alumina, steps (1)-(2) are to acidify the surface of the powdered aluminum oxide to form a hydrated hydroxyl state, which is convenient for the subsequent addition of alkaline compounds and silicon sources for silicon modification.
[0068] In the present invention, the type of the acidic compound has a wide selection range. Preferably, the acidic compound is selected from at least one of hydrochloric acid, nitric acid, sulfuric acid and phosphoric acid. In the present invention, the acidic compound exists in the form of an aqueous solution, and preferably the concentration of the acidic compound in the acidic compound solution is 1-50wt%.
[0069] In the present invention, the first mixing method has a wide range of selection, as long as the aluminum source, the acidic compound and water are mixed. Preferably, in step (1), the first mixing conditions include: temperature of 15-40°C, preferably 20-30°C; rotation speed of 100-1000rpm, preferably 300-1000rpm; time of 0.1-5h, preferably 0.1-2h.
[0070] In the present invention, the molding method has a wide range of choices. Preferably, in step (2), the molding method includes but is not limited to oil-ammonia droplet molding, spray drying molding, and extrusion molding.
[0071] In the present invention, the first drying is to remove water from the first mixture. Preferably, in step (2), the first drying conditions include: temperature of 80-120°C, time of 90-110°C, and time of 1-20h, preferably 1-12h.
[0072] In the present invention, the first drying method has a wide range of options, as long as the conditions of the first drying meet the above-mentioned limitations. Preferably, the first drying method includes but is not limited to spray drying, blast drying, vacuum drying, etc.
[0073] In some embodiments of the present invention, preferably, in step (2), the conditions of the first calcination include: a temperature of 700-1200°C, preferably 800-1000°C; a time of 1-10 hours, preferably 1-5 hours. In the present invention, the first calcination is carried out in a muffle furnace or a tube furnace, and the calcination atmosphere is a non-reducing gas, preferably at least one of air, nitrogen and argon.
[0074] In the present invention, in step (3), the shaped alumina is first dissolved in water, an alkaline compound is added to adjust the pH, and then a silicon source is added for a second mixing, in order to obtain polyhydroxy silicic acid and / or hydroxy hydrated silicon.
[0075] In some embodiments of the present invention, preferably, the pH condition is 8-12, for example, 8, 9, 10, 10.5, 11, 11.5, 12, and any value in the range consisting of any two values, preferably 10.5-11.5.
[0076] In some embodiments of the present invention, preferably, the shaped alumina calculated as Al2O3 and the shaped alumina calculated as SiO x The weight ratio of the silicon source is 5-9:1-5, preferably 7-8:2-3; wherein 1≤x≤2.
[0077] In the present invention, the type of silicon source has a wide range of choices. Preferably, the silicon source is a soluble silicon salt, preferably selected from organic silicon salts and / or inorganic silicon salts, including but not limited to at least one of tetraethyl orthosilicate, tetramethylsilicon, silicon oxide aerogel and silicon tetrachloride.
[0078] In the present invention, unless otherwise specified, solubility means being easily soluble in water, or being easily soluble in water with the help of an auxiliary agent.
[0079] In some embodiments of the present invention, preferably, in step (3), the alkaline compound is selected from at least one of ammonium carbonate, ammonium bicarbonate and aqueous ammonia.
[0080] In some embodiments of the present invention, preferably, in step (3), the conditions for the second mixing include: temperature of 20-70°C, preferably 25-60°C; rotation speed of 100-1000 rpm, preferably 300-1000 rpm; time of 1-20h, preferably 6-12h.
[0081] In the present invention, in step (4), the solid-liquid separation method has a wide range of selection, as long as the second mixture is subjected to solid-liquid separation to obtain a silicon-modified alumina precursor; the solid-liquid separation method includes but is not limited to filtration, sedimentation, etc.
[0082] In the present invention, the second drying is intended to remove the residual moisture in the silicon-modified alumina precursor. Preferably, in step (4), the conditions of the second drying include: temperature of 80-120°C, time of 90-110°C, and time of 1-20h, preferably 1-12h.
[0083] In the present invention, the second drying method has a wide range of options, as long as the second drying conditions meet the above-mentioned limitations. Preferably, the second drying method includes but is not limited to spray drying, blast drying, vacuum drying, etc.
[0084] In some embodiments of the present invention, preferably, in step (4), the conditions of the second calcination include: a temperature of 400-1000°C, preferably 500-900°C; a time of 1-10h, preferably 1-5h. In the present invention, the second calcination is carried out in a muffle furnace or a tubular furnace, and the calcination atmosphere is a non-reducing gas, preferably at least one of air, nitrogen and argon.
[0085] In the present invention, the preparation method of the catalyst has a wide range of choices, as long as the catalyst meets the above definition. Preferably, the catalyst is prepared by the following method: a soluble metal salt is loaded on the surface of the carrier, and the obtained catalyst precursor is subjected to a third drying and a third calcination in sequence to obtain the catalyst.
[0086] In some embodiments of the present invention, preferably, the loading amount of the soluble metal salt in terms of metal element is 0.1-10wt%, for example, 0.1wt%, 0.5wt%, 1wt%, 1.5wt%, 2wt%, 5wt%, 10wt%, and any value in the range of any two values, preferably 0.5-5wt%. In the present invention, the loading amount is based on the total weight of the catalyst.
[0087] In the present invention, the loading method has a wide range of choices, as long as the loading amount of the soluble metal salt meets the above definition. Preferably, the loading method is selected from the group consisting of impregnation method and sedimentation precipitation method.
[0088] In the present invention, when the loading method is impregnation, it is necessary to prepare an impregnation solution containing the soluble metal salt. According to the different amounts of the impregnation solution, the impregnation method is selected from the excess impregnation method and the saturation impregnation method; according to the different ways of impregnation, the impregnation method is selected from the immersion impregnation method and the spray impregnation method. It is easy for those skilled in the art to understand that a catalyst with a specific loading amount can be obtained by adjusting and controlling the concentration, amount or amount of the impregnation solution.
[0089] In some embodiments of the present invention, when the loading method is impregnation, the solvent in the impregnation solution containing the soluble metal salt includes but is not limited to water, ammonia water, and hydrochloric acid. The present invention does not limit the concentration of the soluble metal salt in the impregnation solution containing the soluble metal salt.
[0090] In some embodiments of the present invention, when the loading method is a deposition precipitation method, the solvent in the impregnation solution containing the soluble metal salt includes but is not limited to water. The present invention does not limit the concentration of the soluble metal salt in the impregnation solution containing the soluble metal salt.
[0091] In some embodiments of the present invention, preferably, the soluble metal salt is selected from hydrochloride, sulfate, nitrate, acetate containing at least one of Pt, Pd, Rh, Ir, Ru and Ni, preferably selected from nitrate, sulfate and nitrate containing Pt and / or Pd. In the present invention, the soluble metal salt includes but is not limited to Ni(NO3)2, PdCl2, H2PtCl6, Pd(NO3)2, RuCl3, iridium acetate.
[0092] In some embodiments of the present invention, preferably, the conditions for the third drying include: temperature of 80-120° C., time of 90-110° C., and time of 1-20 h, preferably 1-12 h.
[0093] In the present invention, the third drying method has a wide range of options, as long as the third drying conditions meet the above-mentioned limitations. Preferably, the third drying method includes but is not limited to spray drying, blast drying, vacuum drying, etc.
[0094] In some embodiments of the present invention, preferably, the conditions of the third calcination include: temperature of 400-800°C, time of 450-750°C, time of 1-10h, preferably 1-5h. In the present invention, the third calcination is carried out in a muffle furnace or a tube furnace, and the calcination atmosphere includes but is not limited to air, nitrogen, H2 / N2 atmosphere, etc.
[0095] The present invention provides a preferred method for preparing a supported catalyst, the preparation method comprising:
[0096] (1) performing a first mixing of an aluminum source, an acidic compound, and water to obtain a first mixture;
[0097] (2) subjecting the first mixture to molding, first drying and first calcination in sequence to obtain molded alumina;
[0098] (3) dissolving the shaped alumina in water, first adding an alkaline compound to adjust the pH to 7-12, and then adding a silicon source for a second mixing to obtain a second mixture;
[0099] (4) subjecting the second mixture to solid-liquid separation, and subjecting the obtained silicon-modified alumina precursor to a second drying and a second calcination in sequence to obtain silicon-modified alumina;
[0100] (5) loading a soluble metal salt on the surface of the carrier, and sequentially performing a third drying and a third calcination on the obtained catalyst precursor to obtain a catalyst;
[0101] The B acid density of the silicon-modified alumina is ≤2 μmol / g, preferably 0-2 μmol / g, more preferably 0-1.4 μmol / g, and most preferably 0-0.5 μmol / g.
[0102] In some embodiments of the present invention, when the solvent is selected from alcohols (e.g., methanol), and the carrier in the supported catalyst is selected from silicon-modified alumina with a B acid density ≤2 μmol / g, the reaction temperature is 100-150°C, preferably 100-120°C, and the selectivity of monophenylaminocaprolactam is higher.
[0103] In some embodiments of the present invention, when the solvent is selected from non-alcohols (for example, heteroatom-containing cycloalkanes, heteroatom-containing alkanes, esters, etc.), and the carrier in the supported catalyst is selected from silicon-modified alumina with a B acid density of ≤2 μmol / g, the reaction temperature is 30-80°C, preferably 50-70°C, and the selectivity of monophenylaminocaprolactam is higher.
[0104] The second aspect of the present invention provides a use of monobenzylaminocaprolactam prepared by the preparation method provided in the first aspect as a polymerization monomer in the preparation of functional nylon-6.
[0105] The third aspect of the present invention provides a functional nylon-6, wherein the functional nylon-6 contains the monobenzylaminocaprolactam prepared by the preparation method provided by the first aspect.
[0106] The monobenzylaminocaprolactam prepared by the preparation method provided by the present invention is used as a polymerization monomer in the preparation of functional nylon-6, and the obtained polymer material may have a long branched chain or a network structure, and has potential antibacterial properties, wear resistance, fluorescence, impact resistance, flame retardancy and the like.
[0107] In some embodiments of the present invention, preferably, based on the total weight of the functional nylon-6, the doping amount of monobenzylaminocaprolactam is ≥ 5wt%, for example, 5wt%, 10wt%, 20wt%, 30wt%, and any value in the range of any two values, preferably 10-30wt%. The preferred conditions are adopted so that the glass transition temperature (Tm) of the functional nylon-6 is gradually reduced, that is, the functional nylon-6 provided by the present invention has amorphous characteristics.
[0108] According to a particularly preferred embodiment of the present invention, a method for preparing monobenzylaminocaprolactam comprises: contacting and reacting aminocaprolactam and / or its derivatives with benzaldehyde in the presence of a supported catalyst and a solvent to obtain monobenzylaminocaprolactam;
[0109] The reaction conditions include: temperature of 60-120°C; time of 1-3h; hydrogen pressure of 0.5-5MPa;
[0110] Wherein, the mass ratio of the aminocaprolactam and / or its derivatives to benzaldehyde is 1:0.4-1.2; the mass ratio of the aminocaprolactam and / or its derivatives to the catalyst is 1:0.5-2;
[0111] Wherein, in the supported catalyst, the carrier is selected from silicon-modified alumina with a B acid density of 0-0.5 μmol / g, the active component is selected from Pt and / or Pd, and the dispersion of the active component is 20-80%; based on the total weight of the supported catalyst, the active component content is 0.5-5wt%;
[0112] The silicon-modified alumina comprises silicon and alumina; wherein the silicon-to-alumina ratio of the silicon-modified alumina is less than 1, the silicon is connected to the surface of the alumina through a Si-O-Al chemical bond, and adjacent silicon on the surface of the alumina is connected through a Si-O-Si chemical bond; based on the total weight of the silicon-modified alumina, the content of the alumina is 50-90wt%; and the content of the SiO x The silicon content is 10-50wt%, wherein 1≤x≤2;
[0113] The specific surface area of the silicon-modified alumina is 120-200 m 2 / g; average pore size is 15-25nm; wear index is 1-15%; crushing strength is 70-130N / cm.
[0114] The present invention will be described in detail below through examples.
[0115] The physical properties of the catalysts prepared in Preparation Examples 1-20 are listed in Table 1.
[0116] Preparation Example 1
[0117] (1) 80 g of an aluminum source (pseudo-boehmite), 5 g of an acidic compound (30 wt % dilute nitric acid) and 800 mL of water were first mixed in a 1500 mL stirred tank (temperature: 25° C., rotation speed: 600 rpm, time: 1 h) to obtain a first mixture;
[0118] (2) the first mixture is spray-dried (temperature: 100° C., time: 5 h), and then calcined in a muffle furnace at 800° C. for 3 h in static air to obtain microspherical aluminum oxide;
[0119] (3) dissolving the above-mentioned shaped alumina in 800 mL of water, first adding an alkaline compound (ammonia water) to adjust the pH to 10, and then adding 60 g of a silicon source (ethyl orthosilicate) for a second mixing (temperature of 25° C., rotation speed of 600 rpm, time of 12 h) to obtain a second mixture;
[0120] (4) subjecting the second mixture to solid-liquid separation, and drying the obtained silicon-modified alumina precursor in a vacuum drying oven at 100° C. for 5 h, and then calcining in a muffle furnace at 600° C. for 3 h in static air to obtain microspherical silicon-modified alumina as carrier AS-1;
[0121] (5) A Pd(NH3)4Cl2 solution prepared with 30 wt% ammonia water was impregnated onto the surface of the above-mentioned carrier by an excess impregnation method to obtain a catalyst precursor with a Pd loading of 10 wt%. The catalyst precursor was dried at 100°C in a vacuum drying oven for 5 h and then calcined at 500°C in a muffle furnace for 3 h in static air to obtain a microspherical catalyst Pd / AS-1.
[0122] Among them, the TEM image of catalyst Pd / AS-1 is as follows Figure 2 As shown by Figure 2 It can be seen that the active component Pd in the catalyst Pd / AS-1 is uniformly loaded on the surface of the carrier;
[0123] Among them, the pyridine infrared characterization spectrum of the carrier AS-1 in the catalyst Pd / AS-1 is as follows Figure 3 As shown by Figure 3It can be seen that carrier AS-1 has extremely low B acid sites;
[0124] Among them, the transmission infrared spectrum of carrier AS-1 is as follows Figure 4 As shown in (a), Figure 4 (a) It can be seen that the signal peaks at wavenumbers 1066cm-1 and 1160cm-1 are the vibration absorption peaks of Si-O-Si and Si-O-Al bonds, respectively, indicating that the silicon in the carrier AS-1 is bonded to the alumina through chemical bonds, and the adjacent silicon on the surface of the alumina is SiO x (1≤x≤2) exists in the form of clusters.
[0125] Preparation Example 2
[0126] (1) 50 g of an aluminum source (pseudo-boehmite), 10 g of an acidic compound (5 wt % dilute nitric acid) and 800 mL of water were first mixed in a 1500 mL stirred tank (temperature: 20° C., rotation speed: 500 rpm, time: 1 h) to obtain a first mixture;
[0127] (2) the first mixture is spray-dried (temperature: 100° C., time: 5 h), and then calcined in a muffle furnace at 1000° C. for 1 h in static air to obtain microspherical aluminum oxide;
[0128] (3) dissolving the above-mentioned shaped alumina in 800 mL of water, first adding an alkaline compound (ammonium bicarbonate) to adjust the pH to 9, and then adding 50 g of a silicon source (silicon oxide aerogel) for a second mixing (temperature of 25° C., rotation speed of 500 rpm, time of 8 h) to obtain a second mixture;
[0129] (4) subjecting the second mixture to solid-liquid separation, and drying the obtained silicon-modified alumina precursor in a vacuum drying oven at 100° C. for 5 h, and then calcining in a tubular furnace at 800° C. for 2 h in a nitrogen atmosphere to obtain microspherical silicon-modified alumina as carrier AS-2;
[0130] (5) A Ni(NO3)2 solution was prepared with deionized water and impregnated onto the surface of the above-mentioned carrier by an excess impregnation method to obtain a catalyst precursor with a Ni loading of 6 wt%. The catalyst precursor was dried at 100°C in a vacuum drying oven for 5 h and then calcined at 500°C in static air in a muffle furnace for 3 h to obtain a microspherical catalyst Ni / AS-2.
[0131] Preparation Example 3
[0132] (1) 20 g of an aluminum source (aluminum oxyhydroxide), 1 g of an acidic compound (30 wt % dilute hydrochloric acid) and 800 mL of water were first mixed in a 1500 mL stirred tank (temperature: 30° C., rotation speed: 500 rpm, time: 1 h) to obtain a first mixture;
[0133] (2) Extruding the first mixture, drying it with forced air (temperature of 100° C. for 5 h), and calcining it in a muffle furnace at 800° C. for 3 h to obtain strip-shaped aluminum oxide;
[0134] (3) dissolving the above-mentioned shaped alumina in 800 mL of water, first adding an alkaline compound (ammonia water) to adjust the pH to 10, and then adding 56 g of a silicon source (silicon tetrachloride) for a second mixing (temperature of 50° C., rotation speed of 500 rpm, time of 10 h) to obtain a second mixture;
[0135] (4) The second mixture was subjected to solid-liquid separation, and the obtained silicon-modified alumina precursor was dried in a blast oven at 100° C. for 5 h, and then calcined in a tubular furnace at 600° C. for 6 h in a nitrogen atmosphere to obtain strip-shaped silicon-modified alumina as carrier AS-3;
[0136] (5) Prepare H2PtCl6 solution with deionized water, impregnate it onto the surface of the above-mentioned carrier by saturation impregnation method to obtain a catalyst precursor with a Pt loading of 2wt%. After drying at 100°C in a vacuum drying oven for 5 hours, calcining at 500°C in a tubular furnace in a H2 / N2 atmosphere for 3 hours to obtain a strip catalyst Pt / AS-3.
[0137] Preparation Example 4
[0138] (1) 50 g of an aluminum source (pseudo-boehmite), 2 g of an acidic compound (50 wt % dilute phosphoric acid) and 800 mL of water were first mixed in a 1500 mL stirred tank (temperature: 25° C., rotation speed: 800 rpm, time: 1 h) to obtain a first mixture;
[0139] (2) forming the first mixture into balls by drop molding, drying with forced air (temperature of 100° C. for 5 h), and calcining in a muffle furnace at 1000° C. for 2 h to obtain small spherical aluminum oxide;
[0140] (3) dissolving the above-mentioned shaped alumina in 800 mL of water, first adding an alkaline compound (ammonia water) to adjust the pH to 10, and then adding 48 g of a silicon source (ethyl orthosilicate) for a second mixing (temperature of 35° C., rotation speed of 500 rpm, time of 6 h) to obtain a second mixture;
[0141] (4) The second mixture was subjected to solid-liquid separation, and the obtained silicon-modified alumina precursor was dried in a blast oven at 100° C. for 5 h, and then calcined in a tubular furnace at 800° C. for 3 h in a nitrogen atmosphere to obtain small spherical silicon-modified alumina as a carrier AS-4;
[0142] (5) A Pd(NH3)4(NO3)2 solution was prepared with 30 wt% ammonia water and impregnated onto the surface of the above-mentioned carrier by an excess impregnation method to obtain a catalyst precursor with a Pd loading of 2 wt%. The catalyst precursor was dried at 100°C for 5 h in a vacuum drying oven and then calcined at 500°C in a tubular furnace in a H2 / N2 atmosphere for 3 h to obtain a spherical catalyst Pd / AS-4.
[0143] Preparation Example 5
[0144] (1) 80 g of an aluminum source (γ-alumina), 4 g of an acidic compound (25 wt % dilute sulfuric acid) and 800 mL of water were first mixed in a 1500 mL stirred tank (temperature: 25° C., rotation speed: 600 rpm, time: 1 h) to obtain a first mixture;
[0145] (2) Extruding the first mixture, drying it with forced air (temperature of 100° C. for 5 h), and calcining it in a muffle furnace at 800° C. for 3 h to obtain strip-shaped aluminum oxide;
[0146] (3) dissolving the above-mentioned shaped alumina in 800 mL of water, first adding an alkaline compound (ammonia water) to adjust the pH to 8, and then adding 60 g of a silicon source (ethyl orthosilicate) for a second mixing (temperature of 25° C., rotation speed of 600 rpm, time of 5 h) to obtain a second mixture;
[0147] (4) The second mixture was subjected to solid-liquid separation, and the obtained silicon-modified alumina precursor was dried in a blast oven at 100° C. for 5 h, and then calcined in a tubular furnace at 600° C. for 3 h in a nitrogen atmosphere to obtain strip-shaped silicon-modified alumina as carrier AS-5;
[0148] (5) A PdCl2 solution was prepared with 36 wt% hydrochloric acid and impregnated onto the surface of the carrier by an excess impregnation method to obtain a catalyst precursor with a Pd loading of 10 wt%. The catalyst precursor was dried at 100°C for 5 h in a vacuum drying oven and then calcined at 500°C in a tubular furnace in a H2 / N2 atmosphere for 3 h to obtain a strip catalyst Pd / AS-5.
[0149] Preparation Example 6
[0150] (1) 60 g of an aluminum source (aluminum oxyhydroxide), 5 g of an acidic compound (10 wt % dilute phosphoric acid) and 800 mL of water were first mixed in a 1500 mL stirred tank (temperature: 25° C., rotation speed: 500 rpm, time: 1 h) to obtain a first mixture;
[0151] (2) the first mixture is spray-dried (temperature: 100° C., time: 5 h), and then calcined in a muffle furnace at 900° C. for 3 h in static air to obtain microspherical aluminum oxide;
[0152] (3) The shaped alumina was dissolved in 800 mL of water, an alkaline compound (ammonia water) was added to adjust the pH to 9, and then 28 g of a silicon source (ethyl orthosilicate) was added to perform a second mixing (temperature of 25° C., rotation speed of 500 rpm, time of 9 h) to obtain a second mixture;
[0153] (4) The second mixture was subjected to solid-liquid separation, and the obtained silicon-modified alumina precursor was dried in a blast oven at 100° C. for 5 h, and then calcined in a tubular furnace at 800° C. for 6 h in a nitrogen atmosphere to obtain microspherical silicon-modified alumina as a carrier AS-6;
[0154] (5) A RuCl3 solution was prepared with deionized water and impregnated onto the surface of the above-mentioned carrier by a deposition precipitation method to obtain a catalyst precursor with a loading of 0.5 wt% Ru. The catalyst precursor was dried at 100°C in a vacuum drying oven for 5 h and then calcined at 500°C in a muffle furnace for 3 h in static air to obtain a microspherical catalyst Ru / AS-6.
[0155] Preparation Example 7
[0156] (1) 80 g of an aluminum source (γ-alumina), 50 g of an acidic compound (20 wt % dilute nitric acid) and 800 mL of water were first mixed in a 1500 mL stirred tank (temperature: 25° C., rotation speed: 800 rpm, time: 1 h) to obtain a first mixture;
[0157] (2) the first mixture is spray-dried (temperature: 100° C., time: 5 h), and then calcined in a muffle furnace at 1000° C. for 1 h in static air to obtain microspherical aluminum oxide;
[0158] (3) dissolving the above-mentioned shaped alumina in 800 mL of water, first adding an alkaline compound (ammonium bicarbonate) to adjust the pH to 7.5, and then adding 70 g of a silicon source (ethyl orthosilicate) for a second mixing (temperature of 40° C., rotation speed of 800 rpm, time of 8 h) to obtain a second mixture;
[0159] (4) The second mixture was subjected to solid-liquid separation, and the obtained silicon-modified alumina precursor was dried in a blast oven at 100° C. for 5 h, and then calcined in a tubular furnace at 800° C. for 6 h in a nitrogen atmosphere to obtain microspherical silicon-modified alumina as a carrier AS-7;
[0160] (5) An iridium acetate solution was prepared with deionized water and impregnated onto the surface of the carrier by a deposition precipitation method to obtain a catalyst precursor with an Ir loading of 0.2 wt%. The catalyst precursor was dried at 100° C. for 5 h in a vacuum drying oven and then calcined at 600° C. in a muffle furnace for 3 h in static air to obtain a microspherical catalyst Ir / AS-7.
[0161] Preparation Example 8
[0162] (1) 80 g of an aluminum source (aluminum oxyhydroxide), 5 g of an acidic compound (20 wt % dilute sulfuric acid) and 800 mL of water were first mixed in a 1500 mL stirred tank (temperature: 25° C., rotation speed: 600 rpm, time: 1 h) to obtain a first mixture;
[0163] (2) the first mixture is formed into balls by drop molding, dried by blast drying (temperature is 100° C., time is 5 h), and then calcined in a muffle furnace at 900° C. for 2 h to obtain small spherical aluminum oxide;
[0164] (3) dissolving the above-mentioned shaped alumina in 800 mL of water, first adding an alkaline compound (ammonia water) to adjust the pH to 10, and then adding 50 g of a silicon source (silicon oxide aerogel) for a second mixing (temperature of 25° C., rotation speed of 600 rpm, time of 12 h) to obtain a second mixture;
[0165] (4) The second mixture was subjected to solid-liquid separation, and the obtained silicon-modified alumina precursor was dried in a blast oven at 100° C. for 5 h, and then calcined in a muffle furnace at 600° C. for 4 h in air to obtain small spherical silicon-modified alumina as carrier AS-8;
[0166] (5) RhCl3 solution was prepared with deionized water and impregnated onto the surface of the above-mentioned carrier by a deposition precipitation method to obtain a catalyst precursor with a Rh loading of 2 wt%. The catalyst precursor was dried at 100°C for 5 h in a vacuum drying oven and then calcined at 400°C in a muffle furnace for 5 h in static air to obtain a microspherical catalyst Rh / AS-8.
[0167] Preparation Example 9
[0168] 800 mL of deionized water, 80 g of pseudo-boehmite and 10 g of a 10 wt% dilute nitric acid aqueous solution were mixed in a 1500 mL stirred tank (temperature 25° C., rotation speed 800 rpm, time 5 h), the obtained mixture was subjected to solid-liquid separation, the obtained solid was spray-dried, and then calcined in a muffle furnace at 800° C. for 3 h in static air to obtain microspherical alumina as the carrier Ac-9;
[0169] A Pd(NH3)4Cl2 solution was prepared with 30wt% ammonia water and impregnated onto the surface of the above-mentioned carrier by excessive impregnation method to obtain a catalyst precursor with a Pd loading of 1wt%. The catalyst precursor was dried at 100°C in a vacuum drying oven for 5 hours and then calcined at 500°C in static air in a muffle furnace for 3 hours to obtain a microspherical catalyst Pd / Ac-9.
[0170] Among them, the pyridine infrared characterization spectrum of the carrier Ac-9 in the catalyst Pd / Ac-9 is as follows Figure 3 As shown by Figure 3 It can be seen that the carrier Ac-9 has a higher B acid site.
[0171] Among them, the transmission infrared spectrum of the carrier Ac-9 is as follows Figure 4 As shown in (b), Figure 4 (b) It can be seen that the wave number is 1066cm -1 and 1160cm -1 There are no signal peaks at all, indicating that there are no Si-O-Si and Si-O-Al bonds in the carrier Ac-9.
[0172] Preparation Example 10
[0173] 800 mL of deionized water, 80 g of pseudo-boehmite and 20 g of a 5 wt% dilute nitric acid aqueous solution were mixed in a 1500 mL stirring kettle (temperature 25° C., rotation speed 800 rpm, time 5 h), 60 g of tetraethyl orthosilicate was added, ammonia water was added to adjust the pH to 12, and the mixture was stirred at 25° C. for 12 h. The obtained mixture was spray dried and calcined in a muffle furnace at 800° C. for 3 h in static air to obtain microspherical modified alumina as a carrier Ac-10;
[0174] A Pd(NH3)4Cl2 solution was prepared with 30wt% ammonia water and impregnated onto the surface of the above-mentioned carrier by excessive impregnation method to obtain a catalyst precursor with a Pd loading of 10wt%. The catalyst precursor was dried at 100°C in a vacuum drying oven for 5 hours and then calcined at 500°C in static air in a muffle furnace for 3 hours to obtain a microspherical catalyst Pd / Ac-10.
[0175] Among them, the pyridine infrared characterization spectrum of the carrier Ac-10 in the catalyst Pd / Ac-10 is as follows Figure 3 As shown by Figure 3 It can be seen that the carrier Ac-10 has a higher B acid site.
[0176] Preparation Example 11
[0177] The method of Preparation Example 1 is followed, except that the active ingredients are different, namely,
[0178] In step (5), a 5 wt % platinum ammonia solution is impregnated onto the surface of the carrier by an excess impregnation method to obtain a catalyst precursor with a Pt loading of 5 wt %. The catalyst precursor is dried at 100° C. for 5 h in a vacuum drying oven and then calcined at 500° C. in a muffle furnace at static air for 3 h to obtain a microspherical catalyst Pt / AS-1.
[0179] Preparation Example 12
[0180] The method of Preparation Example 1 is followed, except that the active ingredients are different, namely,
[0181] In step (5), a 10 wt% RuCl3 solution is prepared with deionized water and impregnated onto the surface of the carrier by saturation impregnation to obtain a catalyst precursor with a loading of 1 wt% Ru. The catalyst precursor is dried at 100°C in a vacuum drying oven for 5 h and then calcined at 500°C in a muffle furnace for 3 h in static air to obtain a microspherical catalyst Ru / AS-1.
[0182] Preparation Example 13
[0183] The method of Preparation Example 1 is followed, except that the active ingredients are different, namely,
[0184] In step (5), a 25 wt% Ni(NO3)2 solution is prepared with deionized water and impregnated onto the surface of the above-mentioned carrier by a deposition precipitation method to obtain a catalyst precursor with a loading of 1 wt% Ni. The catalyst precursor is dried at 100°C in a vacuum drying oven for 5 h and then calcined at 500°C in a muffle furnace for 3 h in static air to obtain a microspherical catalyst Ni / AS-1.
[0185] Preparation Example 14
[0186] The method of Example 1 is followed, except that the active ingredients are different, i.e.,
[0187] In step (5), a 20 wt% RhCl3 solution is prepared with deionized water and impregnated onto the surface of the carrier by an excess impregnation method to obtain a catalyst precursor with a loading of 1 wt% Rh. The catalyst precursor is dried at 100°C in a vacuum drying oven for 5 h and then calcined at 500°C in a muffle furnace for 3 h in static air to obtain a microspherical catalyst Rh / AS-1.
[0188] Preparation Example 15
[0189] A 6wt% Pt(NH3)4(NO3)2 solution prepared in deionized water was impregnated onto the SiO2 surface by the excess impregnation method to obtain a catalyst precursor with a Pt loading of 1wt%. After drying at 100°C for 5 hours in a forced air drying oven, the catalyst was calcined at 500°C in a muffle furnace for 3 hours in static air to obtain the catalyst Pt / SiO2.
[0190] Preparation Example 16
[0191] A 10wt% RhCl3 solution prepared in deionized water was impregnated onto the Al2O3 surface by excess impregnation method to obtain a catalyst precursor with a loading of 1wt% Rh. After drying at 100°C for 5h in a forced air drying oven, the catalyst was calcined at 500°C in a N2 atmosphere in a tubular furnace for 3h to obtain the catalyst Rh / Al2O3.
[0192] Preparation Example 17
[0193] A 20wt% H2PtCl4 solution prepared with 37wt% hydrochloric acid was impregnated onto the TiO2 surface by excess impregnation method to obtain a catalyst precursor with a Pt loading of 2wt%. The catalyst was dried at 100°C for 5h in a forced air drying oven and then calcined at 400°C in a muffle furnace for 3h in static air to obtain the catalyst Pt / TiO2.
[0194] Preparation Example 18
[0195] A 10wt% Pt(NH3)4(NO3)2 solution prepared in deionized water was impregnated onto the surface of the HY molecular sieve by the excess impregnation method to obtain a catalyst precursor with a Pt loading of 1wt%. After being dried at 100°C for 5 hours in a forced air drying oven, the catalyst was calcined at 500°C in a muffle furnace for 3 hours in static air to obtain the catalyst Pt / HY.
[0196] Preparation Example 19
[0197] A 20wt% PdCl2 solution prepared with 37wt% hydrochloric acid was impregnated onto the surface of activated carbon by excess impregnation method to obtain a catalyst precursor with a loading of 1wt% Pd. After drying at 100°C for 5h in a forced air drying oven, it was calcined at 500°C in a tubular furnace in a N2 atmosphere for 3h to obtain the catalyst Pd / C.
[0198] Preparation Example 20
[0199] A 6wt% Pt(NH3)4(NO3)2 solution prepared in deionized water was impregnated onto the surface of the HZSM-5 molecular sieve by the excess impregnation method to obtain a catalyst precursor with a Pt loading of 1wt%. After drying at 100°C for 5 hours in a forced air drying oven, the catalyst was calcined at 400°C in a muffle furnace for 3 hours in static air to obtain the catalyst Pd / HZSM-5.
[0200] Table 1
[0201]
[0202] Note: * refers to silicon content in SiO x , where 1≤x≤2.
[0203] Table 1
[0204]
[0205] It can be seen from the results in Table 1 that, compared with Preparation Examples 9-10 and Preparation Examples 15-20, the carriers in the catalysts prepared in Preparation Examples 1-8 and Preparation Examples 11-14 are all silicon-modified alumina, and the silicon-modified alumina satisfies a specific structure, that is, the silicon-to-aluminum ratio of the silicon-modified alumina is less than 1, the silicon in the silicon-modified alumina is connected to the surface of the alumina through Si-O-Al chemical bonds, and the adjacent silicon on the surface of the alumina is connected through Si-O-Si chemical bonds; it also has a lower B acid density, a lower wear index, a better crushing strength, a better specific surface area and a better average pore size.
[0206] Example 1
[0207] In the presence of 40 mL of methanol and 0.2 g of catalyst Pd / AS-1, 0.4 g of aminocaprolactam and 0.4 g of benzaldehyde are reacted in a batch autoclave, wherein the reaction conditions include: temperature of 120° C., hydrogen pressure of 1 MPa, and time of 3 h to obtain a reaction product, wherein the reaction product includes monobenzylaminocaprolactam, bisbenzylaminocaprolactam and a hydrogenation by-product (benzyl alcohol);
[0208] Among them, gas chromatography was used to analyze the catalytic reaction results, and the test results are listed in Table 2.
[0209] Specifically, the reaction product was detected by filtering and separating the reaction solution and the catalyst, adding a certain amount of n-decane as an internal standard, mixing the internal standard and the reaction filtrate evenly, and performing gas phase analysis and quantification (Angilent GC 7890B; separation column: PONA column (0.32 mm × 30 m);
[0210]
[0211] Wherein, the mass of converted aminocaprolactam = the mass of aminocaprolactam – the residual mass of aminocaprolactam.
[0212]
[0213] The yield of benzylaminocaprolactam=the conversion rate of aminocaprolactam×the selectivity of benzylaminocaprolactam×100%.
[0214]
[0215] Embodiment 2-20
[0216] According to Example 1, the difference is that the catalyst type is different, that is,
[0217] The catalyst in Example 1 was replaced by the catalysts of Preparation Examples 2-20, and the test results obtained are listed in Table 2.
[0218] Table 2
[0219]
[0220]
[0221] Note: 1- refers to the conversion rate of aminocaprolactam, %; 2- refers to the yield of monobenzylaminocaprolactam, %.
[0222] It can be seen from the data in Table 2 that the method for preparing monobenzylaminocaprolactam provided by the present invention has a high raw material conversion rate and product selectivity, especially by adjusting the type of carrier and the content of active components in the catalyst, as well as the dosage ratio of the reactants, it is more conducive to improving the catalytic effect of the catalyst and obtaining a high yield of monobenzylaminocaprolactam.
[0223] Examples 21-27
[0224] According to Example 1, the difference is that the process parameters are different, that is,
[0225] The process parameters of Example 1 were replaced with the process parameters in Table 3, and the obtained test results are listed in Table 4.
[0226] Table 3
[0227]
[0228] Table 4
[0229]
[0230] Note: 1- refers to the conversion rate of aminocaprolactam, %; 2- refers to the yield of monobenzylaminocaprolactam, %.
[0231] It can be seen from the data in Table 3-4 that when methanol is used as the solvent, the ideal monobenzylaminocaprolactam selectivity can be obtained by using Pd / AS-1 catalyst under high temperature reaction conditions (100-150°C), while under milder reaction conditions (30-80°C), using non-alcohol solvents (for example, tetrahydrofuran, 1,4-dioxane, ethyl acetate, dimethyl sulfoxide, DMF, etc.), and using Pd / AS-1 to obtain the ideal monobenzylaminocaprolactam selectivity.
[0232] Test Case
[0233] The monobenzylaminocaprolactam prepared in Example 1 is used to prepare functional nylon-6. Based on the total weight of the functional nylon-6, the doping amounts of the monobenzylaminocaprolactam are 10wt%, 20wt% and 30wt%, respectively, to obtain functional nylon-6 with different doping amounts (i.e., 10wt% B-N6, 20wt% B-N6, 30wt% B-N6).
[0234] Among them, the glass transition temperature curves of functional nylon-6 with different doping amounts are shown in the figure below: Figure 5 As shown by Figure 5 It can be seen that as the doping amount of monobenzylaminocaprolactam in the functional nylon-6 gradually increases, the glass transition temperature (Tm) of the functional nylon-6 gradually decreases, that is, the functional nylon-6 provided by the present invention has amorphous characteristics.
[0235] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing monobenzylaminocaprolactam, characterized in that: The preparation method comprises: in the presence of a catalyst and a solvent, aminocaprolactam and / or its derivatives are contacted with benzaldehyde and reacted to obtain monobenzylaminocaprolactam.
2. The preparation method according to claim 1, wherein The reaction conditions include: temperature of 30-150°C; time of 0.5-16h; hydrogen pressure of 0.1-10MPa; Preferably, the reaction conditions include: temperature of 60-120° C.; time of 1-3 h; and hydrogen pressure of 0.5-5 MPa.
3. The preparation method according to claim 1 or 2, wherein The mass ratio of aminocaprolactam and / or its derivatives to benzaldehyde is 1:0.2-2, preferably 1:0.4-1.2; And / or, the mass ratio of the aminocaprolactam and / or its derivatives to the catalyst is 1:0.1-10, preferably 1:0.5-2; And / or, the mass ratio of the aminocaprolactam and / or its derivatives to the solvent is 1:20-200, preferably 1:40-100.
4. The preparation method according to any one of claims 1 to 3, wherein The aminocaprolactam and / or its derivatives are selected from aminocaprolactam and / or aminocaprolactam salts, preferably at least one selected from DL-α-amino-ε-caprolactam, DL-α-amino-ε-caprolactam hydrochloride, DL-α-amino-ε-caprolactam sulfate and DL-α-amino-ε-caprolactam nitrate; And / or, the solvent is selected from organic solvents, preferably at least one selected from organic alcohols, heteroatom-containing cycloalkanes, heteroatom-containing alkanes, esters and aromatic hydrocarbons.
5. The preparation method according to any one of claims 1 to 4, wherein: The catalyst is a supported metal catalyst, and the supported catalyst comprises a support and an active component supported on the support; Preferably, based on the total weight of the catalyst, the content of the carrier is 90-99.9wt%, preferably 95-99.5wt%; the content of the active component is 0.1-10wt%, preferably 0.5-5wt%; Preferably, the carrier is selected from at least one of activated carbon, oxides, molecular sieves and modified oxides; Preferably, the active component is selected from at least one of Pt, Pd, Rh, Ir, Ru and Ni, preferably Pt and / or Pd; Preferably, the dispersion degree of the active ingredient is ≥20%, preferably 20-80%.
6. The preparation method according to claim 5, wherein: The carrier is selected from modified oxides, preferably selected from silicon-modified oxides, and more preferably selected from silicon-modified alumina with a B acid density of ≤2 μmol / g; Preferably, the B acid density of the silicon-modified alumina is 0-2 μmol / g, preferably 0-1.4 μmol / g, and more preferably 0-0.5 μmol / g; Preferably, the silicon-modified alumina comprises silicon and alumina; wherein the silicon-alumina ratio of the silicon-modified alumina is less than 1, the silicon is connected to the surface of the alumina via a Si-O-Al chemical bond, and adjacent silicon on the surface of the alumina is connected via a Si-O-Si chemical bond; Preferably, based on the total weight of the silicon-modified alumina, the content of the alumina is 50-90wt%; x The silicon content is 10-50wt%, wherein 1≤x≤2; Preferably, the specific surface area of the silicon-modified alumina is 100-220 m 2 / g, preferably 120-200m 2 / g; average pore size is 10-30nm, preferably 15-25nm; wear index is 1-20%, preferably 1-15%; crushing strength is 50-150N / cm, preferably 70-130N / cm.
7. The preparation method according to claim 6, wherein: The silicon-modified alumina is prepared by the following method: (1) performing a first mixing of an aluminum source, an acidic compound, and water to obtain a first mixture; (2) subjecting the first mixture to molding, first drying and first calcination in sequence to obtain molded alumina; (3) dissolving the shaped alumina in water, first adding an alkaline compound to adjust the pH to 7-12, and then adding a silicon source for a second mixing to obtain a second mixture; (4) subjecting the second mixture to solid-liquid separation, and subjecting the obtained silicon-modified alumina precursor to a second drying and a second calcination in sequence to obtain the silicon-modified alumina.
8. The preparation method according to any one of claims 5 to 7, wherein: The catalyst is prepared by the following method: a soluble metal salt is loaded on the surface of the carrier, and the obtained catalyst precursor is subjected to a third drying and a third calcination in sequence to obtain the catalyst; Preferably, the loading amount of the soluble metal salt calculated as the metal element is 0.1-10wt%, preferably 0.5-5wt%; Preferably, the loading method is selected from an impregnation method and a deposition precipitation method; Preferably, the soluble metal salt is selected from chlorates, nitrates, sulfates and acetates containing at least one of Pt, Pd, Rh, Ir, Ru and Ni.
9. Use of the monobenzylaminocaprolactam prepared according to the preparation method according to any one of claims 1 to 8 as a polymerization monomer in the preparation of functional nylon-6.
10. A functional nylon-6, characterized in that: The functional nylon-6 contains monobenzylaminocaprolactam prepared by the preparation method according to any one of claims 1 to 8.
Citation Information
Patent Citations
Method for synthesizing DL-alpha-amino caprolactam
CN102093292A
Sulfonamide derivatives
CN101035765A
Novel substituted tetrahydronaphthalenes, process for the preparation thereof and the use thereof as medicaments
CN101784536A
Alpha-(N-benzyl)amino-epsilon-caprolactam compound as well as preparation method and application thereof
CN103694174A
Alpha-(N-disubstituent) amino-epsilon-caprolactam compound as well as preparation method and application thereof
CN104387323A