Nitrogen and phosphorus-containing double-active-center polyaryl cyclic amine polymer, anion exchange membrane and preparation method and application of anion exchange membrane
By introducing polyaryl cyclic amine polymers containing nitrogen and phosphorus dual active centers into anion exchange membranes and using quaternary phosphonium salt copolymerization, the ionic conductivity and mechanical properties of anion exchange membranes are improved, solving the problems of insufficient stability and performance in existing technologies and enabling efficient application under alkaline conditions.
Patent Information
- Application Number
- CN202411093440.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-09
AI Technical Summary
The ionic conductivity, mechanical properties and chemical stability of existing anion exchange membrane materials need to be improved, especially the performance of quaternary ammonium salt anion exchange membranes under alkaline conditions is still not ideal.
By employing polyaryl cyclic amine polymers containing nitrogen and phosphorus dual active centers, and through the introduction of quaternary phosphonium salts and copolymerization methods, the types and ratios of comonomers are adjusted to improve the ionic conductivity and mechanical properties of anion exchange membranes, thereby enhancing their stability under alkaline conditions.
It improves the ionic conductivity and mechanical properties of anion exchange membranes, enhances their stability under alkaline conditions, and makes them suitable for various applications, such as hydrogen fuel cells and flow batteries.
Smart Images

Figure CN118994541A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a nitrogen- and phosphorus-containing dual-active-center polyaryl cyclic amine polymer and anion exchange membrane, a preparation method thereof and applications in the field of ion transmission or separation, and in particular to the structural design of materials such as polyaryl piperidine, polyaryl quinine and polyaryl tropine, belonging to the technical field of anion exchange membrane materials. Background Art
[0002] Hydrogen energy is a clean energy source with advantages such as high combustion calorific value and no pollution from combustion products. Hydrogen production by water electrolysis is currently the most effective hydrogen production technology. Among them, anion exchange membrane water electrolysis technology combines the advantages of traditional alkaline liquid electrolyte water electrolysis and proton exchange membrane water electrolysis. Non-precious metal catalysts such as Ni, Co, and Fe can be used in alkaline media, and the advantages of anion exchange membranes are similar to those of proton exchange membranes, which can avoid dealkalization of product gases. The alkaline system also avoids corrosion problems and greatly reduces equipment costs. Hydrogen fuel cell technology has always been considered the ultimate solution to solve the future human energy crisis using hydrogen energy. Hydrogen fuel cells are mainly composed of anode and cathode plates, catalysts, gas diffusion layers, and ion exchange membranes, which directly convert the chemical energy of hydrogen and oxygen into electrical energy. Among the many types of fuel cells, anion exchange membrane fuel cells have received widespread attention in recent decades due to their low cost, environmental friendliness, and corrosion resistance. In addition, flow batteries are also a new type of electrochemical energy storage technology. The positive and negative electrolytes are separated and circulated separately. They have the characteristics of high capacity, wide application range, and long cycle life. In addition, anion exchange membranes are also required in fields such as electrocatalytic carbon dioxide reduction, metal-air batteries, capacitors, and the chlor-alkali industry, and the improvement of efficiency also greatly depends on high-performance anion exchange membranes.
[0003] As one of the core components of the above-mentioned technologies, the anion conductivity, durability and mechanical properties of the anion exchange membrane (AEM) are crucial. According to different functional groups, AEM can be divided into quaternary ammonium salt anion exchange membrane, imidazole anion exchange membrane, guanidine salt anion exchange membrane, etc. The quaternary ammonium salt type is favored because of its low cost and good stability, but its ion conductivity, mechanical properties and durability still need to be improved. The key to improving the mechanical properties and durability of the membrane still lies in the design of the polymer skeleton. Another key factor restricting the performance of anion exchange membranes is their low ion conductivity level. Previously, patents have reported phosphorus-containing anion exchange membranes, but their conductivity is too low (only 58mS cm at room temperature). -1 ) limits its further application.
[0004] At present, the skeletons of most commercially available anion exchange membranes are mainly polyetheretherketone, polysulfone, polybenzimidazole, etc., and their ion conductivity, chemical stability and mechanical properties under alkaline conditions still need to be further improved. In recent years, the polyarylcyclic amine anion exchange membranes have effectively improved the stability of the membranes, especially the recently developed polyarylpiperidine, polyarylquinine, polyaryltropine and other structures. Due to their simple synthesis process, low cost and excellent performance, they have attracted widespread attention and have great development potential. However, the structural types of this type of anion exchange membrane materials are still very limited, and the mechanical properties and ion conductivity also need to be further improved. Summary of the invention
[0005] The present invention is made based on the inventor's discovery and recognition of the following facts and problems: the electrical conductivity, mechanical properties and chemical stability of the current anion exchange membrane materials need to be improved.
[0006] The present invention aims to solve one of the technical problems in the related art to a certain extent. To this end, the present invention proposes a nitrogen-phosphorus dual-active center polyaryl cyclic amine polymer, anion exchange membrane and its preparation method and application, based on the strong stability of polyaryl cyclic amine membranes under alkaline conditions and their flexible structural designability, and introducing quaternary phosphonium salts into them by direct copolymerization, and by adjusting the types and proportions of copolymer monomers, different uses of anion exchange membranes are achieved, thereby improving the ionic conductivity, mechanical properties and stability of the anion exchange membrane.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] The first aspect of the present invention is to provide a phosphorus-containing polyaryl cyclic amine polymer, containing nitrogen and phosphorus dual active centers, and having at least one of the structural formulas (1) to (4):
[0009]
[0010] in is a benzene ring, naphthalene or binaphthyl;
[0011] wherein R is selected from the group consisting of polyarylpiperidines of the formula or polyarylquinine of the formula Or polyaryltropine of the following formula Any one of; X - It is an anion;
[0012] The molar ratio of the phosphorus-containing groups is 1% to 50%.
[0013] The present invention provides the above-mentioned polymer containing triphenylphosphine, 1,2-bis(diphenylphosphine)ethane, racemic BINAP, R-type BINAP or S-type BINAP, wherein the chemical formula of the polymer with BINAP configuration is as shown in formula (5) to (7):
[0014]
[0015]
[0016] In the chemical formula, y is the molar ratio of phosphorus-containing groups in the polymer, and its value is 1% to 50%.
[0017] The nitrogen- and phosphorus-containing dual-active-center polyaryl cyclic amine polymer designed and synthesized by the present invention has high ion conductivity. The polymer can be prepared into a large-area, high-strength membrane with controllable size and thickness through a film-forming method such as phase inversion or industrial coating, thereby accurately designing and preparing anion exchange membranes that can meet different needs in industrial production.
[0018] The second aspect of the present invention is to provide a method for preparing the above-mentioned nitrogen- and phosphorus-containing dual-active-center polyaryl cyclic amine polymer, comprising the following steps:
[0019] Step 1, adding a phosphorus-containing monomer, an aromatic hydrocarbon compound and a carbonyl compound to an organic solvent, reacting under the condition of strong acid catalysis, and neutralizing, washing and drying after the reaction to obtain a first polymer;
[0020] Step 2, the first polymer obtained in step 1 is reacted with a halogenated hydrocarbon through quaternization and quaternization to obtain a second polymer, namely the nitrogen- and phosphorus-containing dual-active-center polyaryl cyclic amine polymer.
[0021] Preferably, the phosphorus-containing monomer in step 1 is triphenylphosphine, 1,2-bis(diphenylphosphino)ethane, 2,2'-bis(diphenylphosphino)-1,1'-binaphthyl, (R)-(+)-2,2'-bis(diphenylphosphino)-1,1'-binaphthyl or (S)-(-)-2,2'-bis(diphenylphosphino)-1,1'-binaphthyl; the amount of the phosphorus-containing monomer can be adjusted so that the molar ratio of the phosphorus-containing groups in the final product polymer is 1% to 50%; the quaternary phosphonium salt, as a cationic group, can attract and fix negatively charged ions in the ion exchange membrane, can effectively interact with hydroxide ions to form stable ion pairs, and at the same time form hydrophilic regions in the membrane through self-assembly or other interactions, and these hydrophilic regions are interconnected to form continuous ion transmission channels, thereby reducing collisions and obstacles of ions during transmission. Thanks to the high stability of quaternary phosphonium salts in alkaline environments, good ion conductivity and their optimization effect on the phase separation structure and ion transport channels within the membrane, quaternary phosphonium salt cationic groups show higher stability in alkaline environments compared to traditional quaternary ammonium salt cationic groups.
[0022] Preferably, the aromatic compound in step 1 is selected from at least one of biphenyl, p-terphenyl, 9,9-dimethylfluorene, dibenzofuran, dibenzothiophene or other analogs;
[0023] Preferably, the carbonyl compound in step 1 is selected from at least one of 1-methyl-4-piperidone, 3-quinuclidine, tropinone or other analogs. Piperidone, quinuclidine, tropinone and the like exhibit high alkaline stability due to their low ring strain and ability to form a stable conformation. Polyaryl polymers also have high stability in an alkaline environment. In particular, the polyarylquinine structure is selected. Since its cationic group is a quinine unit, the activation energy required for alkaline degradation is very high, thus solving the problem of insufficient stability of the cationic group. At the same time, the conductivity of the quinine-based phosphorus-containing polyarylcyclic amine anion exchange membrane can reach up to 200 mS cm -1 above;
[0024] Further preferably, the reaction temperature of step 1 is 0-25° C., with a better reaction effect at 5° C., and the reaction time is 2-48 hours. As the copolymerization ratio of phosphorus-containing monomers in the system increases, the reaction time needs to be adjusted or extended accordingly.
[0025] Polyaryl polymers have a large number of rigid aromatic rings in their molecular chains. Due to effects such as π-π stacking, the binding force between polymer molecular chains is enhanced. They are very stable under alkaline conditions and are difficult to degrade. The phosphorus-containing ligands used in the synthesis process all have units such as benzene rings and binaphthyl rings with electron-rich groups, which are also very stable under alkaline conditions. The polymer skeleton prepared in this way has good stability under alkaline conditions, which can solve the problem of easy degradation of ion exchange membranes in the prior art.
[0026] In some embodiments, the strong acid used in step 1 is trifluoroacetic acid and trifluoromethanesulfonic acid, and the strong acid catalyzed reaction process is stirring at low temperature until it becomes viscous.
[0027] Preferably, the molar ratio of the aromatic hydrocarbon compound to the carbonyl compound reactant is 1:(1-2).
[0028] Preferably, the halogenated hydrocarbon in step 2 is methyl iodide, ethyl bromide or propyl bromide.
[0029] Preferably, the reaction temperature in step 2 is room temperature, and the reaction time is 24 to 72 hours.
[0030] Preferably, the mass ratio of the halogenated hydrocarbon added in step 2 to the first polymer is (2-3):1.
[0031] The third aspect of the present invention is an anion exchange membrane prepared based on the above-mentioned nitrogen- and phosphorus-containing dual-active-center polyaryl cyclic amine polymer or the above-mentioned preparation method.
[0032] The fourth aspect of the present invention is a method for preparing the above-mentioned anion exchange membrane, which comprises dissolving the aforementioned nitrogen- and phosphorus-containing dual-active-center polyaryl cyclic amine polymer in a solvent and casting it into a membrane, evaporating and drying it, and then immersing it in an anion solution to carry out ion exchange, thereby obtaining the nitrogen- and phosphorus-containing dual-active-center polyaryl cyclic amine anion exchange membrane.
[0033] Wherein, the anion solution is I - Br - , Cl - OH - 、HCO3 - or other chemically acceptable anion solutions; the ion exchange temperature is 25 to 80° C., and the exchange time is 24 to 96 hours.
[0034] The invention also discloses the application of the anion exchange membrane in ion transmission.
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] The nitrogen- and phosphorus-containing dual-active-center cyclic amine polymer proposed by the present invention introduces a quaternary phosphonium salt into a polyaryl cyclic amine anion exchange membrane, and the content of the quaternary phosphonium salt is regulated (1% to 50%) by regulating the amount of the phosphorus-containing monomer, thereby forming nitrogen- and phosphorus-containing dual cationic groups as ion transport exchange sites, thereby improving the stability of the cationic groups in the anion exchange membrane, improving the ion exchange capacity and ion conductivity of the anion exchange membrane, and improving the conductivity of the anion exchange membrane; polyaryl is used as the skeleton of the anion exchange membrane, thereby further improving the mechanical properties of the skeleton of the anion exchange membrane; polyaryl polymers such as piperidone, quinuclidine and tropinone also have high stability in an alkaline environment, so that the anion exchange membrane prepared by the present invention is not easy to decompose under alkaline conditions and has durability.
[0037] The preparation method of phosphorus-containing polyaryl cyclic amines provided by the present invention firstly utilizes an aromatic compound monomer containing phosphorus element to react with an aromatic hydrocarbon compound (such as biphenyl, p-terphenyl, 9,9-dimethylfluorene, dibenzofuran, dibenzothiophene, etc.), 1-methyl-4-piperidone or 3-quinuclidine ketone or tropine ketone under acidic conditions in an organic solvent to prepare several types of polyaryl piperidine, polyaryl quinine, and polyaryl tropine materials containing phosphorus element, and then obtains them through quaternization and quaternization, and the obtained products have excellent ion transport performance. The present invention has simple synthesis process, low cost, and high conductivity of the prepared membrane, so it has broad industrial application prospects.
[0038] The anion exchange membrane prepared based on the nitrogen- and phosphorus-containing dual-active-center cyclic amine polymer has all the advantages and technical effects of the polymer. In some embodiments, by adjusting the type and proportion of the comonomer, different uses of the anion exchange membrane can be achieved.
[0039] The preparation method of the anion exchange membrane proposed by the present invention comprises dissolving a nitrogen- and phosphorus-containing dual-active-center cyclic amine polymer in a solvent to prepare a solution, and using different anion solutions to prepare anion exchange membranes suitable for different purposes, such as a prepared hydroxide-type anion exchange membrane can be applied to a hydrogen fuel cell, and a prepared bicarbonate-type anion exchange membrane can be applied to a liquid flow battery, etc. In addition, thanks to the fact that the anion exchange membrane used in the present invention is rich in aromatic monomers and has strong mechanical structural stability, a membrane material with excellent mechanical structural stability can be prepared without adopting a special treatment method in the film-forming process, so that the preparation method has a wide application prospect. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 This is a schematic diagram of the synthesis of the phosphorus-containing polyaryl piperidine prepared in Example 1 of the present invention.
[0041] Figure 2 This is the FT-IR image of the phosphorus-containing polyaryl piperidine prepared in Example 1 of the present invention.
[0042] Figure 3 This is an FT-IR image of the phosphorus-containing polyarylpiperidine anion exchange membrane prepared in Example 1 of the present invention.
[0043] Figure 4 This is a conductivity picture of the phosphorus-containing polyarylpiperidine anion exchange membrane prepared in Example 1 of the present invention.
[0044] Figure 5 This is a schematic diagram of the synthesis of the phosphorus-containing polyaryl piperidine prepared in Example 2 of the present invention.
[0045] Figure 6 This is the FT-IR image of the phosphorus-containing polyaryl piperidine prepared in Example 2 of the present invention.
[0046] Figure 7 This is an FT-IR image of the phosphorus-containing polyarylpiperidine anion exchange membrane prepared in Example 2 of the present invention.
[0047] Figure 8 This is a conductivity picture of the phosphorus-containing polyarylpiperidine anion exchange membrane prepared in Example 2 of the present invention.
[0048] Fig. 9 This is a schematic diagram of the synthesis of phosphorus-containing polyaryl piperidine prepared in Example 3 of the present invention.
[0049] Fig.10This is the FT-IR image of the phosphorus-containing polyaryl piperidine prepared in Example 3 of the present invention.
[0050] Fig.11 This is an FT-IR image of the phosphorus-containing polyarylpiperidine anion exchange membrane prepared in Example 3 of the present invention.
[0051] Fig.12 This is a conductivity picture of the phosphorus-containing polyarylpiperidine anion exchange membrane prepared in Example 3 of the present invention.
[0052] Fig.13 The present invention provides the structural formula of the phosphorus-containing polyaryl cyclic amine polymer and the anion exchange membrane prepared by the present invention. DETAILED DESCRIPTION
[0053] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0054] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0055] All the reagents used in the examples are commercial reagents, analytically pure 99.9%, without further treatment. The present invention is further described in detail below using specific embodiments in conjunction with the accompanying drawings:
[0056] Example 1
[0057] Step 1: Preparation of racemic phosphorus-containing polyaryl piperidine (M-BINAP-PAP-3%)
[0058] 2,2'-bis(diphenylphosphine)-1,1'-binaphthyl (93.4mg, 0.15mmol), p-terphenyl (1117mg, 4.85mmol) were added to a 25ml round-bottom flask, dichloromethane (5ml) was added as a solvent, and 1-methyl-4-piperidone (0.7ml) was added. The flask was then immersed in an ice bath and stirred for ten minutes. Trifluoroacetic acid (0.4ml) and trifluoromethanesulfonic acid (4.5ml) were added in sequence. Then stirred at low temperature for 4-8 hours, and the reaction stopped when the viscous liquid in the bottle could not be stirred. After the reaction stopped, the liquid was poured into a mixed solution of methanol (100ml) and 1M KOH (100ml), and the solid was completely precipitated. Then it was washed with 1M KOH and water several times until it was neutral, and vacuum dried at 100℃ for 12h to obtain the product.
[0059] Step 2: Preparation I - Racemic phosphorus-containing polyaryl piperidine (M-BINAP-PAP-3%-I - )
[0060] Weigh 500 mg of the product of step 1 and 400 mg of potassium carbonate in a glass bottle, add 15 ml of DMSO and 0.5 ml of iodomethane, and react at room temperature in the dark for 48 hours. After 48 hours, pour into ethyl acetate to obtain a white solid, wash once with ethyl acetate, wash twice with water, and dry in vacuum at 100°C.
[0061] Step 3: Preparation of OH - Racemic phosphorus-containing polyaryl piperidine anion exchange membrane (M-BINAP-PAP-3%-OH - -AEM)
[0062] Disperse 500 mg of the product obtained in step 2 in 20 ml of DMSO, dissolve it completely by ultrasonication, cast the solution in a flat glass petri dish, dry it at 80°C for 6 h and at 120°C for 12 h to obtain a flat anion exchange membrane. Then soak the membrane in 1 M KOH and perform ion exchange at 80°C for 48 h to obtain OH - type anion exchange membrane.
[0063] The synthesis diagram of phosphorus-containing polyaryl piperidine M-BINAP-PAP-3% prepared in step 1 is as follows Figure 1 shown. Figure 2 The FT-IR (Fourier Transform Infrared spectroscopy, FT-IR) test results show that Figure 2 CP (1490 cm -1 ) and CN(1370cm -1) characteristic peaks, which can prove the successful synthesis of phosphorus-containing polyaryl piperidine.
[0064] Figure 3 is the FTIR of the membrane, Figure 3 It can be found that CP (1490cm -1 ) and CN(1370cm -1 ) characteristic peaks become significantly weaker, which proves the successful formation of quaternary phosphonium salt and quaternary ammonium salt groups.
[0065] pass Figure 4 The anion exchange membrane M-BINAP-PAP-3%-OH - -The conductivity curve of AEM changes with temperature. It is known that the conductivity of the membrane at 80°C is: 180.1mS cm -1 . Anion exchange membrane M-BINAP-PAP-3%-OH - -AEM mechanical properties test shows that the tensile strength of the membrane is above 60MPa, showing excellent mechanical properties. Anion exchange membrane M-BINAP-PAP-3%-OH - - Durability test of AEM, after soaking in 1M KOH for more than 1800h, the conductivity dropped by only 1.5%, showing excellent alkali stability.
[0066] Example 2
[0067] Step 1: Preparation of R-type phosphorus-containing polyaryl piperidine (R-BINAP-PAP-3%)
[0068] (R)-(+)-2,2'-bis(diphenylphosphino)-1,1'-binaphthyl (93.4mg, 0.15mmol), p-terphenyl (1117mg, 4.85mmol), were added to a 25ml round-bottom flask, dichloromethane (5ml) was added as a solvent, and 1-methyl-4-piperidone (0.7ml) was added, and then the flask was immersed in an ice bath and stirred for ten minutes, and trifluoroacetic acid (0.42ml) and trifluoromethanesulfonic acid (4.5ml) were added in sequence. Then stirred at low temperature for 4-8 hours, and the reaction stopped when the viscous liquid in the bottle could not be stirred. After the reaction stopped, the liquid was poured into a mixed solution of methanol (100ml) and 1M KOH (100ml), and the solid was completely precipitated. Then it was washed with 1M KOH and water several times until it was neutral, and vacuum dried at 100℃ for 12h to obtain the product.
[0069] Step 2: Preparation I - R-BINAP-PAP-3%-I - )
[0070] Weigh 500 mg of the product of step 1 and 400 mg of potassium carbonate in a glass bottle, add 15 ml of DMSO and 0.5 ml of iodomethane, and react at room temperature in the dark for 48 hours. After 48 hours, pour into ethyl acetate to obtain a white solid, wash once with ethyl acetate, wash twice with water, and dry in vacuum at 100°C.
[0071] Step 3: Preparation of OH - R-type phosphorus-containing polyaryl piperidine anion exchange membrane (R-BINAP-PAP-3%-OH - -AEM)
[0072] Disperse 500 mg of the product obtained in step 2 in 20 ml of DMSO, dissolve it completely by ultrasonication, cast the solution in a flat glass petri dish, dry it at 80°C for 6 h and at 120°C for 12 h to obtain a flat anion exchange membrane. Then soak the membrane in 1 M KOH and perform ion exchange at 80°C for 48 h to obtain OH - type anion exchange membrane.
[0073] The synthesis diagram of phosphorus-containing polyaryl piperidine R-BINAP-PAP-3% prepared in step 2 is as follows: Figure 5 shown. Figure 6 The FT-IR test results show that Figure 6 CP (1490 cm -1 ) and CN(1370cm -1 ) characteristic peaks, which can prove the successful synthesis of phosphorus-containing polyaryl piperidine.
[0074] Figure 3 For anion exchange membrane R-BINAP-PAP-3%-OH - - FT-IR of AEM, by Figure 7 It can be found that CP (1490cm -1 ) and CN(1370cm -1 ) characteristic peaks become significantly weaker, which proves the successful formation of quaternary phosphonium and quaternary ammonium groups.
[0075] pass Figure 8 The anion exchange membrane R-BINAP-PAP-3%-OH - -The conductivity curve of AEM changes with temperature. It is known that the conductivity of the membrane at 80°C is: 207.1mS cm -1 .
[0076] Example 3
[0077] Step 1: Preparation of S-type phosphorus-containing polyaryl piperidine (S-BINAP-PAP-3%)
[0078] (S)-(-)-2,2'-bis(diphenylphosphine)-1,1'-binaphthyl (93.4mg, 0.15mmol), p-terphenyl (1117mg, 4.85mmol), were added to a 25ml round-bottom flask, dichloromethane (5ml) was added as a solvent, and 1-methyl-4-piperidone (0.7ml) was added. The flask was then immersed in an ice bath and stirred for ten minutes, and trifluoroacetic acid (0.42ml) and trifluoromethanesulfonic acid (4.5ml) were added in sequence. Then, the mixture was stirred at low temperature for 4-8 hours, and the reaction was stopped when the viscous liquid in the bottle could not be stirred. After the reaction stopped, the liquid was poured into a mixed solution of methanol (100ml) and 1M KOH (100ml), and the solid was completely precipitated. Then, the mixture was washed with 1M KOH and water several times until it was neutral, and the product was obtained by vacuum drying at 100℃ for 12h.
[0079] Step 2: Preparation I - S-type phosphorus-containing polyaryl piperidine (S-BINAP-PAP-3%-I - )
[0080] Weigh 500 mg of the product of step 1 and 400 mg of potassium carbonate in a glass bottle, add 15 ml of DMSO and 0.5 ml of iodomethane, and react at room temperature in the dark for 48 hours. After 48 hours, pour into ethyl acetate to obtain a white solid, wash once with ethyl acetate, wash twice with water, and dry in vacuum at 100°C.
[0081] Step 3: Preparation of OH - S-type phosphorus-containing polyaryl piperidine anion exchange membrane (S-BINAP-PAP-3%-OH - -AEM)
[0082] Disperse 500 mg of the product obtained in step 2 in 20 ml of DMSO, dissolve it completely by ultrasonication, cast the solution in a flat glass petri dish, dry it at 80°C for 6 h and at 120°C for 12 h to obtain a flat anion exchange membrane. Then soak the membrane in 1 M KOH and perform ion exchange at 80°C for 48 h to obtain OH - type anion exchange membrane.
[0083] The synthesis diagram of phosphorus-containing polyaryl piperidine S-BINAP-PAP-3% prepared in step 1 is as follows Fig. 9 shown. Fig.10 The FT-IR test results show that Fig.10 CP (1490 cm -1 ) and CN(1370cm -1 ) characteristic peaks, which can prove the successful synthesis of phosphorus-containing polyaryl piperidine.
[0084] Fig.11 For anion exchange membrane S-BINAP-3%-OH - - FT-IR of AEM, by Fig.11 It can be found that CP (1490cm -1 ) and CN(1370cm -1 ) characteristic peaks become significantly weaker, which proves the successful formation of quaternary phosphonium and quaternary ammonium groups.
[0085] pass Fig.12 The anion exchange membrane S-BINAP-3%-OH - -The conductivity curve of AEM changes with temperature. It is known that the conductivity of the membrane at 80°C is: 202.3mS cm -1 .
[0086] Example 4
[0087] Step 1: Preparation of racemic phosphorus-containing polyarylquinine (M-BINAP-PAQ-3%)
[0088] 2,2'-bis(diphenylphosphine)-1,1'-binaphthyl (93.4mg, 0.15mmol), p-terphenyl (1117mg, 4.85mmol) were added to a 25ml round-bottom flask, dichloromethane (5ml) was added as a solvent, and 3-quinuclidine ketone (751mg) was added. The flask was then immersed in an ice bath and stirred for ten minutes, and trifluoromethanesulfonic acid (5ml) was added. Then, the mixture was stirred overnight at low temperature, and the reaction stopped when the viscous liquid in the bottle could not be stirred. After the reaction stopped, the liquid was poured into a mixed solution of methanol (100ml) and 1M KOH (100ml), and the solid was completely precipitated. Then, the mixture was washed with 1M KOH and water several times until it was neutral, and the product was obtained by vacuum drying at 100℃ for 12h.
[0089] Step 2: Preparation I - Racemic phosphorus-containing polyarylquinine (M-BINAP-PAQ-3%-I - )
[0090] Weigh 500 mg of the product of step 1 and 400 mg of potassium carbonate in a glass bottle, add 15 ml of DMSO and 0.5 ml of iodomethane, and react at room temperature in the dark for 48 hours. After 48 hours, pour into ethyl acetate to obtain a white solid, wash once with ethyl acetate, wash twice with water, and dry in vacuum at 100°C.
[0091] Step 3: Preparation of OH - Racemic phosphorus-containing polyarylquinine anion exchange membrane (M-BINAP-PAQ-3%-OH - -AEM)
[0092] Disperse 500 mg of the product obtained in step 2 in 20 ml of DMSO, dissolve it completely by ultrasonication, cast the solution in a flat glass petri dish, dry it at 80°C for 6 h and at 120°C for 12 h to obtain a flat anion exchange membrane. Then soak the membrane in 1 M KOH and perform ion exchange at 80°C for 48 h to obtain OH - type anion exchange membrane.
[0093] Example 5
[0094] Step 1: Preparation of R-type phosphorus-containing polyarylquinine (R-BINAP-PAQ-3%)
[0095] (R)-(+)-2,2'-bis(diphenylphosphino)-1,1'-binaphthyl (93.4mg, 0.15mmol), p-terphenyl (1117mg, 4.85mmol), were added to a 25ml round-bottom flask, dichloromethane (5ml) was added as a solvent, and 3-quinuclidine ketone (751mg) was added. The flask was then immersed in an ice bath and stirred for ten minutes, and trifluoromethanesulfonic acid (5ml) was added. Then, the mixture was stirred overnight at low temperature, and the reaction stopped when the viscous liquid in the bottle could not be stirred. After the reaction stopped, the liquid was poured into a mixed solution of methanol (100ml) and 1M KOH (100ml), and the solid was completely precipitated. Then, the mixture was washed with 1M KOH and water several times until it was neutral, and the product was obtained by vacuum drying at 100℃ for 12h.
[0096] Step 2: Preparation I - R-BINAP-PAQ-3%-I - )
[0097] Weigh 500 mg of the product of step 1 and 400 mg of potassium carbonate in a glass bottle, add 15 ml of DMSO and 0.5 ml of iodomethane, and react at room temperature in the dark for 48 hours. After 48 hours, pour into ethyl acetate to obtain a white solid, wash once with ethyl acetate, wash twice with water, and dry in vacuum at 100°C.
[0098] Step 3: Preparation of OH - R-BINAP-PAQ-3%-OH - -AEM)
[0099] Disperse 500 mg of the product obtained in step 2 in 20 ml of DMSO, dissolve it completely by ultrasonication, cast the solution in a flat glass petri dish, dry it at 80°C for 6 h and at 120°C for 12 h to obtain a flat anion exchange membrane. Then soak the membrane in 1 M KOH and perform ion exchange at 80°C for 48 h to obtain OH - type anion exchange membrane.
[0100] Example 6
[0101] Step 1: Preparation of S-type phosphorus-containing polyarylquinine (S-BINAP-PAQ-3%)
[0102] (S)-(-)-2,2'-bis(diphenylphosphino)-1,1'-binaphthyl (93.4mg, 0.15mmol), p-terphenyl (1117mg, 4.85mmol), were added to a 25ml round-bottom flask, dichloromethane (5ml) was added as a solvent, and 3-quinuclidine ketone (751mg) was added. The flask was then immersed in an ice bath and stirred for ten minutes, and trifluoromethanesulfonic acid (5ml) was added. Then, the mixture was stirred overnight at low temperature, and the reaction stopped when the viscous liquid in the bottle could not be stirred. After the reaction stopped, the liquid was poured into a mixed solution of methanol (100ml) and 1M KOH (100ml), and the solid was completely precipitated. Then, the mixture was washed with 1M KOH and water several times until it was neutral, and the product was obtained by vacuum drying at 100℃ for 12h.
[0103] Step 2: Preparation I - S-BINAP-PAQ-3%-I - )
[0104] Weigh 500 mg of the product of step 1 and 400 mg of potassium carbonate in a glass bottle, add 15 ml of DMSO and 0.5 ml of iodomethane, and react at room temperature in the dark for 48 hours. After 48 hours, pour into ethyl acetate to obtain a white solid, wash once with ethyl acetate, wash twice with water, and dry in vacuum at 100°C.
[0105] Step 3: Preparation of OH - S-type phosphorus-containing polyarylquinine anion exchange membrane (S-BINAP-PAQ-3%-OH - -AEM)
[0106] Disperse 500 mg of the product obtained in step 2 in 20 ml of DMSO, dissolve it completely by ultrasonication, cast the solution in a flat glass petri dish, dry it at 80°C for 6 h and at 120°C for 12 h to obtain a flat anion exchange membrane. Then soak the membrane in 1 M KOH and perform ion exchange at 80°C for 48 h to obtain OH - type anion exchange membrane.
[0107] Example 7
[0108] Step 1: Preparation of racemic phosphorus-containing polyaryltropine (M-BINAP-PAT-3%)
[0109] 2,2'-bis(diphenylphosphine)-1,1'-binaphthyl (93.4mg, 0.15mmol), p-terphenyl (1117mg, 4.85mmol) were added to a 25ml round-bottom flask, dichloromethane (5ml) was added as a solvent, and tropinone (835.2mg) was added. The flask was then immersed in an ice bath and stirred for ten minutes, and trifluoromethanesulfonic acid (5ml) was added. Then, the mixture was stirred overnight at low temperature, and the reaction stopped when the viscous liquid in the bottle could not be stirred. After the reaction stopped, the liquid was poured into a mixed solution of methanol (100ml) and 1M KOH (100ml), and the solid was completely precipitated. Then, the mixture was washed with 1M KOH and water several times until it was neutral, and the product was obtained by vacuum drying at 100℃ for 12h.
[0110] Step 2: Preparation I - Racemic phosphorus-containing polyaryl tropine (M-BINAP-PAT-3%-I - )
[0111] Weigh 500 mg of the product of step 1 and 400 mg of potassium carbonate in a glass bottle, add 15 ml of DMSO and 0.5 ml of iodomethane, and react at room temperature in the dark for 48 hours. After 48 hours, pour into ethyl acetate to obtain a white solid, wash once with ethyl acetate, wash twice with water, and dry in vacuum at 100°C.
[0112] Step 3: Preparation of OH - Racemic phosphorus-containing polyaryl tropine anion exchange membrane (M-BINAP-PAT-3%-OH - -AEM)
[0113] Disperse 500 mg of the product obtained in step 2 in 20 ml of DMSO, dissolve it completely by ultrasonication, cast the solution in a flat glass petri dish, dry it at 80°C for 6 h and at 120°C for 12 h to obtain a flat anion exchange membrane. Then soak the membrane in 1 M KOH and perform ion exchange at 80°C for 48 h to obtain OH - type anion exchange membrane.
[0114] Example 8
[0115] Step 1: Preparation of R-BINAP-PAT-3%
[0116] (R)-(+)-2,2'-bis(diphenylphosphino)-1,1'-binaphthyl (93.4mg, 0.15mmol), p-terphenyl (1117mg, 4.85mmol), were added to a 25ml round-bottom flask, dichloromethane (5ml) was added as a solvent, and tropinone (835.2mg) was added. The flask was then immersed in an ice bath and stirred for ten minutes, and trifluoromethanesulfonic acid (5ml) was added. Then, the mixture was stirred overnight at low temperature, and the reaction stopped when the viscous liquid in the bottle could not be stirred. After the reaction stopped, the liquid was poured into a mixed solution of methanol (100ml) and 1M KOH (100ml), and the solid was completely precipitated. Then, the mixture was washed with 1M KOH and water several times until it was neutral, and the product was obtained by vacuum drying at 100℃ for 12h.
[0117] Step 2: Preparation I - R-BINAP-PAT-3%-I - )
[0118] Weigh 500 mg of the product of step 1 and 400 mg of potassium carbonate in a glass bottle, add 15 ml of DMSO and 0.5 ml of iodomethane, and react at room temperature in the dark for 48 hours. After 48 hours, pour into ethyl acetate to obtain a white solid, wash once with ethyl acetate, wash twice with water, and dry in vacuum at 100°C.
[0119] Step 3: Preparation of OH - R-BINAP-PAT-3%-OH - -AEM)
[0120] Disperse 500 mg of the product obtained in step 2 in 20 ml of DMSO, dissolve it completely by ultrasonication, cast the solution in a flat glass petri dish, dry it at 80°C for 6 h and at 120°C for 12 h to obtain a flat anion exchange membrane. Then soak the membrane in 1 M KOH and perform ion exchange at 80°C for 48 h to obtain OH - type anion exchange membrane.
[0121] Example 9
[0122] Step 1: Preparation of S-type phosphorus-containing polyaryl tropine (S-BINAP-PAT-3%)
[0123] (S)-(-)-2,2'-bis(diphenylphosphino)-1,1'-binaphthyl (93.4mg, 0.15mmol), p-terphenyl (1117mg, 4.85mmol), were added to a 25ml round-bottom flask, dichloromethane (5ml) was added as a solvent, and tropinone (835.2mg) was added. The flask was then immersed in an ice bath and stirred for ten minutes, and trifluoromethanesulfonic acid (5ml) was added. Then, the mixture was stirred overnight at low temperature, and the reaction stopped when the viscous liquid in the bottle could not be stirred. After the reaction stopped, the liquid was poured into a mixed solution of methanol (100ml) and 1M KOH (100ml), and the solid was completely precipitated. Then, the mixture was washed with 1M KOH and water several times until it was neutral, and the product was obtained by vacuum drying at 100℃ for 12h.
[0124] Step 2: Preparation I - S-BINAP-PAT-3%-I - )
[0125] Weigh 500 mg of the product of step 1 and 400 mg of potassium carbonate in a glass bottle, add 15 ml of DMSO and 0.5 ml of iodomethane, and react at room temperature in the dark for 48 hours. After 48 hours, pour into ethyl acetate to obtain a white solid, wash once with ethyl acetate, wash twice with water, and dry in vacuum at 100°C.
[0126] Step 3: Preparation of OH - S-type phosphorus-containing polyaryl tropine anion exchange membrane (S-BINAP-PAT-3%-OH - -AEM)
[0127] Disperse 500 mg of the product obtained in step 2 in 20 ml of DMSO, dissolve it completely by ultrasonication, cast the solution in a flat glass petri dish, dry it at 80°C for 6 h and at 120°C for 12 h to obtain a flat anion exchange membrane. Then soak the membrane in 1 M KOH and perform ion exchange at 80°C for 48 h to obtain OH - type anion exchange membrane.
[0128] Example 10
[0129] Step 1: Preparation of triphenylphosphine-type polyarylpiperidine (TPP-PAP-3%)
[0130] Triphenylphosphine (39.4 mg, 0.15 mmol) and p-terphenyl (1117 mg, 4.85 mmol) were added to a 25 ml round-bottom flask, dichloromethane (5 ml) was added as a solvent, and 1-methyl-4-piperidone (0.7 ml) was added. The flask was then immersed in an ice bath and stirred for ten minutes. Trifluoroacetic acid (0.4 ml) and trifluoromethanesulfonic acid (4.5 ml) were added in sequence. Then, the mixture was stirred at low temperature for 4-8 hours. The reaction was stopped when the viscous liquid in the bottle could not be stirred. After the reaction stopped, the liquid was poured into a mixed solution of methanol (100 ml) and 1M KOH (100 ml), and the solid was completely precipitated. Then, the mixture was washed with 1M KOH and water several times until it was neutral, and the product was obtained by vacuum drying at 100°C for 12 hours.
[0131] Step 2: Preparation I - Triphenylphosphine polyaryl piperidine (TPP-PAP-3%-I - )
[0132] Weigh 500 mg of the product of step 1 and 400 mg of potassium carbonate in a glass bottle, add 15 ml of DMSO and 0.5 ml of iodomethane, and react at room temperature in the dark for 48 hours. After 48 hours, pour into ethyl acetate to obtain a white solid, wash once with ethyl acetate, wash twice with water, and dry in vacuum at 100°C.
[0133] Step 3: Preparation of OH - Triphenylphosphine polyarylpiperidinium anion exchange membrane (TPP-PAP-3%-OH - -AEM)
[0134] Disperse 500 mg of the product obtained in step 2 in 20 ml of DMSO, dissolve it completely by ultrasonication, cast the solution in a flat glass petri dish, dry it at 80°C for 6 h and at 120°C for 12 h to obtain a flat anion exchange membrane. Then soak the membrane in 1 M KOH and perform ion exchange at 80°C for 48 h to obtain OH - type anion exchange membrane.
[0135] Embodiment 11
[0136] Step 1: Preparation of triphenylphosphine polyarylquinine (TPP-PAQ-3%)
[0137] Triphenylphosphine (39.4 mg, 0.15 mmol) and p-terphenyl (1117 mg, 4.85 mmol) were added to a 25 ml round-bottom flask, dichloromethane (5 ml) was added as a solvent, and 3-quinuclidine ketone (751 mg) was added. The flask was then immersed in an ice bath and stirred for ten minutes, and trifluoromethanesulfonic acid (5 ml) was added. Then, the mixture was stirred overnight at low temperature, and the reaction stopped when the viscous liquid in the bottle could not be stirred. After the reaction stopped, the liquid was poured into a mixed solution of methanol (100 ml) and 1M KOH (100 ml), and the solid was completely precipitated. Then, the mixture was washed with 1M KOH and water several times until it was neutral, and the product was obtained by vacuum drying at 100°C for 12 hours.
[0138] Step 2: Preparation I - Triphenylphosphine polyarylquinine (TPP-PAQ-3%-I - )
[0139] Weigh 500 mg of the product of step 1 and 400 mg of potassium carbonate in a glass bottle, add 15 ml of DMSO and 0.5 ml of iodomethane, and react at room temperature in the dark for 48 hours. After 48 hours, pour into ethyl acetate to obtain a white solid, wash once with ethyl acetate, wash twice with water, and dry in vacuum at 100°C.
[0140] Step 3: Preparation of OH - Triphenylphosphine polyarylquinine anion exchange membrane (TPP-PAQ-3%-OH - -AEM)
[0141] Disperse 500 mg of the product obtained in step 2 in 20 ml of DMSO, dissolve it completely by ultrasonication, cast the solution in a flat glass petri dish, dry it at 80°C for 6 h and at 120°C for 12 h to obtain a flat anion exchange membrane. Then soak the membrane in 1 M KOH and perform ion exchange at 80°C for 48 h to obtain OH - type anion exchange membrane.
[0142] Example 12
[0143] Step 1: Preparation of triphenylphosphine polyaryltropine (TPP-PAT-3%)
[0144] Triphenylphosphine (39.4 mg, 0.15 mmol) and p-terphenyl (1117 mg, 4.85 mmol) were added to a 25 ml round-bottom flask, dichloromethane (5 ml) was added as a solvent, and tropinone (835.2 mg) was added. The flask was then immersed in an ice bath and stirred for ten minutes, and trifluoromethanesulfonic acid (5 ml) was added. Then, the mixture was stirred overnight at low temperature, and the reaction stopped when the viscous liquid in the bottle could not be stirred. After the reaction stopped, the liquid was poured into a mixed solution of methanol (100 ml) and 1 M KOH (100 ml), and the solid was completely precipitated. Then, the mixture was washed with 1 M KOH and water several times until it was neutral, and the product was obtained by vacuum drying at 100 ° C for 12 hours.
[0145] Step 2: Preparation I - Triphenylphosphine polyaryl tropine (TPP-PAT-3%-I - )
[0146] Weigh 500 mg of the product of step 1 and 400 mg of potassium carbonate in a glass bottle, add 15 ml of DMSO and 0.5 ml of iodomethane, and react at room temperature in the dark for 48 hours. After 48 hours, pour into ethyl acetate to obtain a white solid, wash once with ethyl acetate, wash twice with water, and dry in vacuum at 100°C.
[0147] Step 3: Preparation of OH - Triphenylphosphine polyaryl tropine anion exchange membrane (TPP-PAT-3%-OH - -AEM)
[0148] Disperse 500 mg of the product obtained in step 2 in 20 ml of DMSO, dissolve it completely by ultrasonication, cast the solution in a flat glass petri dish, dry it at 80°C for 6 h and at 120°C for 12 h to obtain a flat anion exchange membrane. Then soak the membrane in 1 M KOH and perform ion exchange at 80°C for 48 h to obtain OH - type anion exchange membrane.
[0149] Embodiment 13
[0150] Step 1: Preparation of 1,2-bis(diphenylphosphino)ethane polyarylpiperidine (BDPE-PAP-3%)
[0151] 1,2-bis(diphenylphosphino)ethane (59.8mg, 0.15mmol), p-terphenyl (1117mg, 4.85mmol) were added to a 25ml round-bottom flask, dichloromethane (5ml) was added as a solvent, and 1-methyl-4-piperidone (0.7ml) was added. The flask was then immersed in an ice bath and stirred for ten minutes. Trifluoroacetic acid (0.4ml) and trifluoromethanesulfonic acid (4.5ml) were added in sequence. Then stirred at low temperature for 4-8 hours, and the reaction stopped when the viscous liquid in the bottle could not be stirred. After the reaction stopped, the liquid was poured into a mixed solution of methanol (100ml) and 1M KOH (100ml), and the solid was completely precipitated. Then it was washed with 1M KOH and water several times until it was neutral, and vacuum dried at 100℃ for 12h to obtain the product.
[0152] Step 2: Preparation I - 1,2-Bis(diphenylphosphino)ethane polyarylpiperidinium (BDPE-PAP-3%-I - )
[0153] Weigh 500 mg of the product of step 1 and 400 mg of potassium carbonate in a glass bottle, add 15 ml of DMSO and 0.5 ml of iodomethane, and react at room temperature in the dark for 48 hours. After 48 hours, pour into ethyl acetate to obtain a white solid, wash once with ethyl acetate, wash twice with water, and dry in vacuum at 100°C.
[0154] Step 3: Preparation of OH - 1,2-Bis(diphenylphosphino)ethane polyarylpiperidinium anion exchange membrane (BDPE-PAP-3%-OH - -AEM)
[0155] Disperse 500 mg of the product obtained in step 2 in 20 ml of DMSO, dissolve it completely by ultrasonication, cast the solution in a flat glass petri dish, dry it at 80°C for 6 h and at 120°C for 12 h to obtain a flat anion exchange membrane. Then soak the membrane in 1 M KOH and perform ion exchange at 80°C for 48 h to obtain OH - type anion exchange membrane.
[0156] Embodiment 14
[0157] Step 1: Preparation of 1,2-bis(diphenylphosphino)ethane polyarylquinine (BDPE-PAQ-3%)
[0158] 1,2-bis(diphenylphosphino)ethane (59.8mg, 0.15mmol), p-terphenyl (1117mg, 4.85mmol) were added to a 25ml round-bottom flask, dichloromethane (5ml) was added as a solvent, and 3-quinuclidine ketone (751mg) was added. The flask was then immersed in an ice bath and stirred for ten minutes, and trifluoromethanesulfonic acid (5ml) was added. Then, the mixture was stirred overnight at low temperature, and the reaction stopped when the viscous liquid in the bottle could not be stirred. After the reaction stopped, the liquid was poured into a mixed solution of methanol (100ml) and 1M KOH (100ml), and the solid was completely precipitated. Then, the mixture was washed with 1M KOH and water several times until it was neutral, and the product was obtained by vacuum drying at 100℃ for 12h.
[0159] Step 2: Preparation I - 1,2-Bis(diphenylphosphino)ethane polyarylquinine (BDPE-PAQ-3%-I - )
[0160] Weigh 500 mg of the product of step 1 and 400 mg of potassium carbonate in a glass bottle, add 15 ml of DMSO and 0.5 ml of iodomethane, and react at room temperature in the dark for 48 hours. After 48 hours, pour into ethyl acetate to obtain a white solid, wash once with ethyl acetate, wash twice with water, and dry in vacuum at 100°C.
[0161] Step 3: Preparation of OH - 1,2-Bis(diphenylphosphino)ethane polyarylquinine anion exchange membrane (BDPE-PAQ-3%-OH - -AEM)
[0162] Disperse 500 mg of the product obtained in step 2 in 20 ml of DMSO, dissolve it completely by ultrasonication, cast the solution in a flat glass petri dish, dry it at 80°C for 6 h and at 120°C for 12 h to obtain a flat anion exchange membrane. Then soak the membrane in 1 M KOH and perform ion exchange at 80°C for 48 h to obtain OH - type anion exchange membrane.
[0163] Embodiment 15
[0164] Step 1: Preparation of 1,2-bis(diphenylphosphino)ethane poly(aryl tropine) (BDPE-PAT-3%)
[0165] 1,2-bis(diphenylphosphino)ethane (59.8mg, 0.15mmol), p-terphenyl (1117mg, 4.85mmol) were added to a 25ml round-bottom flask, dichloromethane (5ml) was added as a solvent, and tropinone (835.2mg) was added. The flask was then immersed in an ice bath and stirred for ten minutes, and trifluoromethanesulfonic acid (5ml) was added. Then, the mixture was stirred overnight at low temperature, and the reaction stopped when the viscous liquid in the bottle could not be stirred. After the reaction stopped, the liquid was poured into a mixed solution of methanol (100ml) and 1M KOH (100ml), and the solid was completely precipitated. Then, the mixture was washed with 1M KOH and water several times until it was neutral, and the product was obtained by vacuum drying at 100℃ for 12h.
[0166] Step 2: Preparation I - 1,2-Bis(diphenylphosphino)ethane polyaryltropine (BDPE-PAT-3%-I - )
[0167] Weigh 500 mg of the product of step 1 and 400 mg of potassium carbonate in a glass bottle, add 15 ml of DMSO and 0.5 ml of iodomethane, and react at room temperature in the dark for 48 hours. After 48 hours, pour into ethyl acetate to obtain a white solid, wash once with ethyl acetate, wash twice with water, and dry in vacuum at 100°C.
[0168] Step 3: Preparation of OH - 1,2-Bis(diphenylphosphino)ethane polyaryltropine anion exchange membrane (BDPE-PAT-3%-OH - -AEM)
[0169] Disperse 500 mg of the product obtained in step 2 in 20 ml of DMSO, dissolve it completely by ultrasonication, cast the solution in a flat glass petri dish, dry it at 80°C for 6 h and at 120°C for 12 h to obtain a flat anion exchange membrane. Then soak the membrane in 1 M KOH and perform ion exchange at 80°C for 48 h to obtain OH - type anion exchange membrane.
[0170] The structural formulas of the phosphorus-containing polyaryl cyclic amine polymers and anion exchange membranes prepared in the above examples are as follows: Fig.13 shown.
[0171] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A polyaromatic cyclic amine polymer containing nitrogen and phosphorus dual active centers, characterized in that: Contains nitrogen and phosphorus dual active centers and has at least one of the structural formulas (1) to (4): in is a benzene ring, naphthalene or binaphthyl; wherein R is selected from the group consisting of polyarylpiperidines of the formula or polyarylquinine of the formula Or polyaryltropine of the following formula Any one of; X - It is an anion; The molar ratio of the phosphorus-containing groups is 1% to 50%.
2. The nitrogen- and phosphorus-containing dual-active-center polyaryl cyclic amine polymer according to claim 1, characterized in that: The anion exchange polymer comprises at least one of formulas (5) to (7): In the chemical formula, y is the molar ratio of the phosphorus-containing group, and its value is 1% to 50%.
3. A method for preparing a nitrogen- and phosphorus-containing dual-active-center polyaryl cyclic amine polymer according to claim 1 or claim 2, characterized in that: The following steps are involved: Step 1, adding a phosphorus-containing monomer, an aromatic hydrocarbon compound and a carbonyl compound to an organic solvent, reacting under the condition of strong acid catalysis, and neutralizing, washing and drying after the reaction to obtain a first polymer; Step 2, quaternizing and quaternizing the first polymer with a halogenated hydrocarbon to obtain a second polymer, namely the polyaryl cyclic amine polymer containing nitrogen and phosphorus dual active centers.
4. The method for preparing the nitrogen- and phosphorus-containing dual-active-center polyaryl cyclic amine polymer according to claim 3, characterized in that: The phosphorus-containing monomer in step 1 is triphenylphosphine, 1,2-bis(diphenylphosphino)ethane, 2,2'-bis(diphenylphosphino)-1,1'-binaphthyl, (R)-(+)-2,2'-bis(diphenylphosphino)-1,1'-binaphthyl or (S)-(-)-2,2'-bis(diphenylphosphino)-1,1'-binaphthyl; The aromatic hydrocarbon compound is selected from at least one of biphenyl, p-terphenyl, 9,9-dimethylfluorene, dibenzofuran, and dibenzothiophene; The carbonyl compound is selected from 1-methyl-4-piperidone, 3-quinuclidinone or tropinone.
5. The method for preparing the nitrogen- and phosphorus-containing dual-active-center polyaryl cyclic amine polymer according to claim 3, characterized in that: The reaction temperature of step 1 is 0 to 25° C., and the reaction time is 2 to 48 hours.
6. The method for preparing the nitrogen- and phosphorus-containing dual-active-center polyaryl cyclic amine polymer according to claim 3, characterized in that: The halogenated hydrocarbon in step 2 is methyl iodide, ethyl bromide or propyl bromide, and the mass ratio of the halogenated hydrocarbon to the first polymer is (2-3):
1.
7. The method for preparing the nitrogen- and phosphorus-containing dual-active-center polyaryl cyclic amine polymer according to claim 3, characterized in that: The reaction temperature of step 2 is room temperature, and the reaction time is 24 to 72 hours.
8. A nitrogen- and phosphorus-containing dual-active-center polyaryl cyclic amine anion exchange membrane, characterized in that: The polyaryl cyclic amine polymer containing nitrogen and phosphorus double active centers is prepared by using the polyaryl cyclic amine polymer containing nitrogen and phosphorus double active centers as described in claim 1 or 2 or the polyaryl cyclic amine polymer containing nitrogen and phosphorus double active centers prepared by the preparation method described in any one of claims 3 to 7.
9. A method for preparing the nitrogen- and phosphorus-containing dual-active-center polyaryl cyclic amine anion exchange membrane according to claim 8, characterized in that: The nitrogen-phosphorus dual-active-center polyaryl cyclic amine polymer is dissolved in a solvent and cast into a film, and after evaporation and drying, it is immersed in an anion solution for ion exchange, so as to obtain the nitrogen-phosphorus dual-active-center polyaryl cyclic amine anion exchange membrane; The anion solution is I - Br - , Cl - OH - 、HCO3 - or other chemically acceptable anion solutions; the ion exchange temperature is 25 to 80° C., and the ion exchange time is 24 to 96 hours.
10. Use of the nitrogen-phosphorus dual-active-center polyaryl cyclic amine anion exchange membrane according to claim 8 or the nitrogen-phosphorus dual-active-center polyaryl cyclic amine anion exchange membrane prepared by the preparation method according to claim 9 in ion transport.
Citation Information
Patent Citations
Dibenzofuran-containing polyaryl piperidine anion exchange membrane and preparation method thereof
CN116622042A
Polyaryl quinine polymer, preparation method and anion exchange membrane prepared from polyaryl quinine polymer
CN117106161A
Polyaryl acridine anion exchange membrane with high ionic conductivity and high dimensional stability as well as preparation method and application of polyaryl acridine anion exchange membrane
CN117304536A
Anion exchange membrane with branched structure as well as preparation method and application of anion exchange membrane
CN117467121A
Cross-linked alkaline anion membrane based on cyclodextrin modification as well as preparation method and application of cross-linked alkaline anion membrane
CN118185099A
Cited By
Branched agglomerated aryl cyclamine anion exchange membrane containing multiple cationic groups as well as preparation method and application of branched agglomerated aryl cyclamine anion exchange membrane
CN120900451A