Polyamide-imide containing furan ring structure as well as synthesis method and application of polyamide-imide

The synthesis of PAI through the polycondensation reaction of aromatic diamine and tetracarboxylic acid with a furan ring structure and high-temperature imine synthesis, the high cost and chloride ion residue problems of the acid chloride method are solved, and the green synthesis and high dielectric constant of PAI are achieved. in electronic products.

CN118994579AActive Publication Date: 2024-11-22ZHEJIANG YUANBANG MATERIAL TECH
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202411484281.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-23
Publication Date
2024-11-22
Estimated Expiration
2044-10-23

AI Technical Summary

Technical Problem

The acyl chloride method used in the existing polyamide-imide (PAI) production process has problems such as high cost, equipment corrosion, chloride ion residues and dielectric properties, which limits the development of materials.

Method used

The PAI is synthesized by polycondensation reaction and high-temperature imine synthesis of aromatic diamines and aromatic tetracarboxylic acid using furan ring structure, avoiding the release of HCl and the participation of chloride ions. Water is used as the reaction medium, which simplifies the process steps and improves the Product stability.

Benefits of technology

It realizes green synthesis of PAI, reduces production costs, improves the dielectric constant stability and mechanical properties of the product, and is suitable for the electronic product field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994579A_ABST
    Figure CN118994579A_ABST
Patent Text Reader

Abstract

The invention provides polyamide-imide containing a furan ring structure as well as a synthesis method and application thereof, the polyamide-imide containing the furan ring structure comprises a repetitive structure as shown in a formula I: # imgabs0 #, n is more than 50 and less than 200, and n is an integer; ar is one of substituent groups containing an aromatic ring structure. The technical scheme provided by the invention is short in flow, simple and convenient to operate, free of hydrogen chloride release in the preparation process, and green and friendly; and a film prepared from the polyamide-imide containing the furan ring structure is good in mechanical property and low in dielectric constant, and has huge application potential in the field of electronic products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymers, and in particular relates to a polyamide-imide containing a furan ring structure, a synthesis method and application thereof. Background Art

[0002] Polyamide-imide (PAI for short) is a type of high-temperature resistant thermoplastic engineering plastics with excellent performance. Since the main chain of the molecule contains both heat-resistant imide groups and flexible amide groups, PAI products not only have the heat resistance, low creep, high strength, high modulus, and solvent resistance of polyimide, but also have the excellent mechanical properties and molding processing properties of polyamide. It can be molded by conventional injection molding, extrusion, and compression molding processes. Therefore, it is widely used in aerospace, military equipment, chemical equipment, electronic equipment, and other fields, and has broad development prospects.

[0003] Torlon (polyamide-imide) produced by Amoco Chemicals Co., Ltd. in the United States usually adopts the acyl chloride method, that is, using trimellitic anhydride chloride (TMAc) and aromatic diamine as raw materials, PAI is prepared by condensation in a nitrogen-containing polar organic solvent. The acyl chloride method for producing PAI has been industrialized and the technology is relatively mature, but there are the following problems: (1) The key raw material trimellitic anhydride chloride is expensive and has poor storage stability, and its upstream raw material trimellitic anhydride (TMA) has been identified as a substance of high concern by the European Union due to its respiratory sensitization; (2) The acyl chloride route involves the prepolymerization, powdering, and thermal imidization of polyamic acid. The route is long and the difficulty of controlling the stability of product performance increases; (3) The HCl released during the production process of the acyl chloride method will corrode the equipment and is difficult to separate completely from the product. The residual chloride ions seriously affect the insulation performance of electronic and electrical equipment, and the purification and removal of HCl will also greatly increase the production cost. Especially for electronic materials, the amount of chloride ions in the material directly affects the dielectric constant and dielectric loss factor of the material. These defects have largely become limiting factors in the development of PAI. Summary of the invention

[0004] In view of the above-mentioned shortcomings of the prior art, the object of the present invention is to provide a polyamide-imide containing a furan ring structure and a synthesis method and use thereof, so as to solve the problems in the prior art.

[0005] To achieve the above objectives and other related objectives, the present invention is achieved through the following technical solutions.

[0006] The first aspect of the present invention provides a polyamide-imide containing a furan ring structure, wherein the polyamide-imide comprises a repeating structure as shown in Formula I: Formula I; wherein 50<n<200 and is an integer; Ar is one of the substituents containing an aromatic ring structure.

[0007] Preferably, Ar is selected from one of the following structures: , , , .

[0008] Preferably, the number average molecular weight of the polyamide-imide containing a furan ring structure is 3×10 4 ~1.2×10 5 More preferably, the molecular weight of the polyamide-imide containing a furan ring structure is 3×10 4 ~5.5×10 4 The number average molecular weight is obtained by GPC test. For example, the molecular weight is 3.1×10 4 ~5.5×10 4 , 3.6~5.0×10 4 .

[0009] A second aspect of the present invention provides a method for synthesizing the polyamide-imide containing a furan ring structure as described above, comprising the following steps: 1) contacting an aromatic diamine containing a furan ring structure, an aromatic tetracarboxylic acid, a first catalyst and water to carry out a polycondensation reaction to obtain an aqueous suspension, and dehydrating and drying the aqueous suspension to obtain a polyamic acid containing a furan ring structure; 2) The polyamic acid is subjected to solid phase viscosity enhancement and high temperature imidization to obtain the polyamide-imide containing a furan ring structure.

[0010] In the present application, water is used as the reaction medium. Since the polyamic acid prepared in step 1) has poor solubility in water, the formed polyamic acid suspension is easily dehydrated by centrifugal separation. The steps are simple and the recovery efficiency of the polyamic acid product is high.

[0011] Preferably, the structural formula of the aromatic diamine containing a furan ring structure is as shown in Formula II: Formula II.

[0012] Preferably, the aromatic tetracarboxylic acid is selected from one or more of pyromellitic acid, biphenyltetracarboxylic acid, 3,3',4,4'-dibenzophenonetetracarboxylic acid and 4,4-oxydiphthalic acid.

[0013] Preferably, in step 1), based on the total weight of the aromatic diamine containing a furan ring structure, the aromatic tetracarboxylic acid and water, the water content is 80-90%; and the molar ratio of the aromatic diamine to the aromatic tetracarboxylic acid is 1.01-1.05:1.

[0014] For example, based on the total weight of the aromatic diamine containing a furan ring structure, the aromatic tetracarboxylic acid and water, the water content can be 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%. For example, the molar ratio of the aromatic diamine to the aromatic tetracarboxylic acid can be 1.01:1, 1.02:1, 1.03:1, 1.04:1, 1.05:1.

[0015] Preferably, based on the total weight of the aromatic diamine containing a furan ring structure, the aromatic tetracarboxylic acid and water, the added amount of the first catalyst is 0.2-1.5 wt ‰, such as 0.2-1.0 wt ‰, 1.0-1.5 wt ‰.

[0016] The molar ratio of the aromatic diamine containing a furan ring structure to the aromatic tetracarboxylic acid is not arbitrarily limited. If the content of the aromatic diamine containing a furan ring structure is low, the reaction is incomplete, resulting in a low yield of the product; if the content of the aromatic diamine containing a furan ring structure is too high, the end-capping effect is obvious during the reaction, and only oligomer products can be obtained in the end.

[0017] Preferably, the first catalyst is a hypophosphite catalyst.

[0018] More preferably, the hypophosphite catalyst is selected from one or more of sodium hypophosphite, potassium hypophosphite, calcium hypophosphite and magnesium hypophosphite.

[0019] Preferably, in step 1), the polycondensation reaction includes a first stage and a second stage.

[0020] Preferably, the first stage reaction temperature is 100-150°C, and the first stage reaction time is 3-6h. For example, the reaction temperature may be 100-120°C, 120-150°C, and the reaction time may be 3h, 4h, 5h, or 6h.

[0021] Preferably, the second stage reaction temperature is 130-180°C, and the second stage reaction time is 3-6h. For example, the reaction temperature may be 130-150°C, 140-180°C, and the reaction time may be 3h, 4h, 5h, or 6h.

[0022] Preferably, the pressure of the second stage reaction is 0.5-1.5 MPa. For example, the pressure may be 0.5-1.2 MPa, 1.2-1.5 MPa.

[0023] Preferably, in step 1), the polycondensation reaction is also stirred at a rate of 50 to 400 r / min. For example, the stirring rate may be 50 to 200 r / min or 200 to 400 r / min.

[0024] Preferably, in step 1), the polycondensation reaction is carried out in an inert gas environment.

[0025] Preferably, in step 1), a centrifugal separator is used for the dehydration and drying.

[0026] Preferably, the polycondensation reaction is carried out in a high-pressure polymerization reactor.

[0027] Preferably, in step 2), the temperature of the solid phase viscosity enhancement reaction is 200-260° C. For example, the temperature of the solid phase viscosity enhancement reaction may be 200° C., 210° C., 220° C., 230° C., 240° C., 250° C., or 260° C.

[0028] Preferably, in step 2), the solid phase viscosity enhancement reaction time is 4 to 10 hours. For example, the reaction time can be 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, or 10 hours.

[0029] Preferably, in step 2), the solid phase viscosity increasing reaction is carried out under vacuum conditions, wherein the vacuum degree is 40-80 Pa. For example, the vacuum degree may be 50-60 Pa, 40-60 Pa, or 50-80 Pa.

[0030] Preferably, in step 2), a second catalyst is added during the solid phase viscosity increasing reaction, and the second catalyst is selected from one or more of diisopropylamine, 4-dimethylaminopyridine and triphenylphosphine.

[0031] Preferably, in step 2), based on the total mass of the polyamic acid, the amount of the second catalyst added is 0.2-1.5 wt‰, such as 0.2-1.0 wt‰ or 1.0-1.5 wt‰.

[0032] Preferably, in step 2), a vacuum drum reactor is used to carry out the solid phase viscosity increasing reaction.

[0033] The third aspect of the present invention provides a use of the polyamide-imide containing a furan ring structure as described above in the preparation of a low dielectric film or in the preparation of an electronic product substrate or as an insulating material.

[0034] A fourth aspect of the present invention provides a low dielectric film prepared by using the polyamide-imide containing a furan ring structure as described above.

[0035] Preferably, the polyamide-imide containing a furan ring structure is dissolved in an organic solvent to form a solution, the solution is applied on a glass plate, and dried at high temperature to obtain the low dielectric film. Preferably, the organic solvent includes NMP.

[0036] Preferably, the high temperature drying temperature is 60-300°C.

[0037] Preferably, the dielectric constant of the low dielectric film is 2.6-3.2, such as 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, or 3.2.

[0038] Preferably, the tensile strength of the low dielectric film is 220-290 MPa, such as 220-250 MPa, 240-290 MPa, 230-270 MPa, or 220-280 MPa. Preferably, the elongation at break of the low dielectric film is 2.2-2.7%, such as 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, or 2.7%.

[0039] The beneficial effects of the present invention are as follows: 1) The present invention uses an aromatic diamine containing a furan ring structure and an aromatic tetracarboxylic acid as reaction raw materials, and prepares PAI by polycondensation reaction and high-temperature imidization, thereby abandoning the technical solution of using a halogen-containing monomer as a reaction raw material in the prior art, so that no HCl is released during the reaction process, and the synthesis process is green and friendly.

[0040] 2) In the process of preparing polyamide-imide (PAI) using the technical solution of the present invention, there is no involvement of chloride ions, so the dielectric constant of the product is low and the application prospect in the field of electronic products is broad.

[0041] 3) In this technical solution, the synthesis of polyamide-imide containing a furan ring structure can be completed by only two steps, and the route is short and easy to operate.

[0042] 4) In the present invention, the molecular weight of the polyamide-imide product can be adjusted by changing the process parameters of the solid phase viscosity enhancement, and the distribution coefficient of the molecular weight of the polyamide-imide product can be reduced, and the product properties are more excellent. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 The aromatic diamine containing a furan ring structure used in the present invention is shown 1 H-NMR spectrum.

[0044] Figure 2 The aromatic diamine containing a furan ring structure used in the present invention is shown 13 C-NMR spectrum.

[0045] Figure 3 Shown is the infrared spectrum of the polyamide-imide containing a furan ring structure prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0046] The following is a description of the implementation of the present invention by means of specific embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification.

[0047] Before further describing the specific embodiments of the present invention, it should be understood that the scope of protection of the present invention is not limited to the specific embodiments described below; it should also be understood that the terms used in the examples of the present invention are intended to describe specific embodiments, rather than to limit the scope of protection of the present invention. The test methods in the following examples without specifying specific conditions are generally carried out under conventional conditions or under conditions recommended by the manufacturers.

[0048] When the embodiments give numerical ranges, it should be understood that, unless otherwise specified in the present invention, both endpoints of each numerical range and any numerical value between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those generally understood by those skilled in the art. In addition to the specific methods, equipment, and materials used in the embodiments, according to the grasp of the prior art by those skilled in the art and the record of the present invention, any methods, equipment, and materials of the prior art similar or equivalent to the methods, equipment, and materials described in the embodiments of the present invention can also be used to realize the present invention.

[0049] The present application does not specifically limit the preparation method of the aromatic diamine containing a furan ring structure, as long as the aromatic diamine containing a furan ring structure as shown in Formula II can be obtained, Formula II.

[0050] In the following implementation of the present application, the aromatic diamine containing a furan ring structure used is prepared by the following preparation method, and the specific steps are: a) 90 mmol of triethylamine and 90 mmol of p-nitroaniline are dissolved in 50 mL of DMAc, and stirred at room temperature to completely dissolve. Under a N2 atmosphere, 37.5 mL of a DMAc solution containing 40 mmol of 2,5-furandicarbonyl chloride is added dropwise, and stirred at room temperature for 24 h to obtain a mixed solution. Then, the mixed solution is dropped into water to form a precipitate, and the precipitate is collected by filtration and washed with water, and vacuum dried at 95°C to obtain a dinitro compound.

[0051] b) 3.155 g of the dinitro compound obtained in step a) was taken and dissolved in 30 mL of DMAc, and 65.6 mg of Pd / C catalyst was added to obtain a reaction solution. Then 6 mL of hydrazine hydrate (50%) was slowly dripped into the reaction solution at 100°C, and stirred for 24 h under N2 atmosphere. After the reaction was completed, the Pd / C catalyst was removed by filtration, and the filtrate was dripped into water to produce a yellow precipitate, which was vacuum dried at 60°C overnight to obtain an aromatic diamine containing a furan ring structure as shown in Formula II.

[0052] The applicant uses nuclear magnetic resonance technology to analyze and detect the aromatic diamine containing a furan ring structure, and its NMR spectrum is as follows: Figure 1 and Figure 2 shown.

[0053] Depend on Figure 1 and Figure 2 It can be seen that the above preparation method indeed obtains an aromatic diamine containing a furan ring structure with a structural formula as shown in Formula II.

[0054] Example 1

[0055] The present embodiment provides a method for synthesizing a polyamide-imide containing a furan ring structure, which specifically includes the following steps: 1) dissolving 200.24 g of an aromatic diamine containing a furan ring structure, 148 g of pyromellitic acid (molar ratio of 1.02:1), and 2.9 g (1 wt‰) of sodium hypophosphite in 2554 ml of water, and adding the mixture into a reactor (the reactor is equipped with a mechanical stirrer, a condenser and a thermometer), stirring at a temperature of 120°C, and carrying out a first-stage reaction for 5 hours, with a mechanical stirring speed of 200 r / min.

[0056] After the first stage of reaction, the air in the reactor was replaced by vacuuming and passing high-purity argon gas, and this cycle was repeated 6 times, so that a pressure of 0.2MPa was reserved in the reactor after the replacement step. Under the protection of high-purity argon gas, the temperature in the reactor was increased to 180°C at a heating rate of 2°C / min, the pressure in the reactor was increased to 1.2MPa, the mechanical stirring speed was 200r / min, and the second stage of reaction was carried out for 3 hours to obtain a polyamic acid aqueous suspension.

[0057] After the second stage reaction is completed, when the temperature in the reactor drops to room temperature, the polyamic acid aqueous suspension is discharged from the bottom of the reactor, dehydrated and dried by a centrifugal separator to obtain polyamic acid.

[0058] 2) 300 g of the polyamic acid obtained in step 1) was added to a vacuum drum reactor, imidized at a temperature of 200° C., and viscosity-increasing for 6 h. During the process, vacuum was continuously drawn and water was removed. The vacuum degree of the drum reactor was maintained at 50 Pa to obtain the polyamide-imide containing a furan ring structure. The molecular weight of the polyamide-imide containing a furan ring structure was 3.1×10 4 .

[0059] The polyamide-imide containing furan ring structure prepared in this example was subjected to infrared spectrum analysis. The results are as follows: Figure 3 shown.

[0060] Depend on Figure 3 It can be seen that 3325 cm -1The peak at 1742 cm is the stretching vibration absorption peak of NH in the amide bond; -1 The absorption peak at 1700 cm is the symmetric stretching vibration absorption peak of -CO-N-CO- in the imine ring; -1 The asymmetric stretching vibration absorption peak of -CO-N-CO- in the imine ring is at 1666 cm -1 The peak at 1600 cm is the stretching vibration absorption peak of C=O in the amide bond; -1 and 1500 cm -1 The peak at 1375 cm is the vibration absorption peak of the benzene ring; -1 The peak at 725 cm is the stretching vibration absorption peak of CN in the imine ring; -1 The absorption peak at is the bending vibration of -CO-N-CO- in the imine ring.

[0061] This indicates that the synthesis method provided in this example successfully prepared polyamide-imide containing a furan ring structure.

[0062] Example 2 1) Step 1) is the same as in Example 1, obtaining polyamic acid; 2) 300 g of the polyamic acid obtained in step 1) was added to a vacuum drum reactor, imidized at 240° C., and viscosity-increasing for 7 h. During the process, vacuum was continuously drawn and water was removed. The vacuum degree of the drum reactor was maintained at 60 Pa to obtain the polyamide-imide containing a furan ring structure. The molecular weight of the polyamide-imide containing a furan ring structure was 3.8×10 4 .

[0063] Example 3 1) Step 1) is the same as in Example 1, obtaining polyamic acid; 2) 300 g of the polyamic acid obtained in step 1) and 0.3 g of diisopropylamine were added to a vacuum drum reactor, imidized at a temperature of 260° C., and viscosity increased for 8 h. During the process, vacuum was continuously drawn and water was removed, and the vacuum degree of the drum reactor was maintained at 50 Pa to obtain the polyamide-imide containing a furan ring structure. The molecular weight of the polyamide-imide containing a furan ring structure is 5×10 4 .

[0064] Example 4 1) The raw materials in Example 1 were replaced with: 200.24 g of an aromatic diamine containing a furan ring structure and 191 g of biphenyltetracarboxylic acid (molar ratio of 1.01:1), and 2.6 g (1 wt‰) of sodium hypophosphite were dissolved in 2216 ml of water and added to a reactor, and the remaining steps were exactly the same to obtain polyamic acid; 2) 300 g of the polyamic acid obtained in step 1) was added to a vacuum drum reactor, imidized at 260° C., and viscosity-increasing for 8 h. During the process, vacuum was continuously drawn and water was removed. The vacuum degree of the drum reactor was maintained at 50 Pa to obtain the polyamide-imide containing a furan ring structure. The molecular weight of the polyamide-imide containing a furan ring structure was 3.6×10 4 .

[0065] Example 5 1) Step 1) is the same as step 4 to obtain polyamic acid; 2) 300 g of the polyamic acid obtained in step 1) and 0.3 g of diisopropylamine were added to a vacuum drum reactor, imidized at a temperature of 260° C., and viscosity increased for 8 h. During the process, vacuum was continuously drawn and water was removed, and the vacuum degree of the drum reactor was maintained at 50 Pa to obtain the polyamide-imide containing a furan ring structure. The molecular weight of the polyamide-imide containing a furan ring structure is 5.5×10 4 .

[0066] The applicant also soaked the glass plate in acetone for 1 hour, then rinsed it with deionized water, dried it in an oven, and then added the furan ring structure-containing polyamide-imide prepared in Examples 1 to 5 to NMP to form a PAI solution, wherein the solid content of the PAI solution was 18%. A PAI coating with a thickness of 100 μm was then prepared on the glass plate using a wet film preparation device, and then maintained at 60°C, 80°C, 120°C, 150°C, 200°C, 250°C, and 300°C for 2 hours. After cooling, the glass plate was immersed in deionized water and peeled off to obtain a light yellow PAI film.

[0067] With reference to GB / T 1040.3-2006, the tensile strength and elongation at break of the PAI film were determined using an electronic universal material testing machine, and the dielectric constant was measured using a Concept 40 broadband dielectric tester. The specific results are shown in Table 1 below.

[0068] Table 1 Tensile Strength Elongation at break Dielectric constant Example 1 220 MPa 2.2% 3.2 Example 2 252 MPa 2.4% 3.0 Example 3 276 MPa 2.6% 2.6 Example 4 243 MPa 2.4% 2.9 Example 5 290 MPa 2.7% 3.0 As can be seen from Table 1, the film made from the polyamide-imide containing furan ring structure provided by the present invention has good mechanical properties, a tensile strength of 220 MPa~290 MPa, and an elongation at break of 2.2~2.7%; and a low dielectric constant of 2.6~3.2, and has great application potential in the field of electronic products.

[0069] In summary, the technical solution of the present invention provides a convenient preparation process with a short process and simple operation, and no HCl is released during the preparation process, which is environmentally friendly; and the film made of the polyamide-imide containing a furan ring structure obtained thereby has good mechanical properties and a low dielectric constant, and has great application potential in the field of electronic products.

[0070] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A polyamide-imide containing a furan ring structure, characterized in that: The polyamide-imide comprises a repeating structure as shown in Formula I: Formula I; Wherein, 50<n<200 and is an integer; Ar is one of the substituents containing an aromatic ring structure.

2. The polyamide-imide containing a furan ring structure according to claim 1, characterized in that: The Ar is selected from one of the following structures: 、 、 、 ; And / or, the number average molecular weight of the polyamide-imide containing furan ring structure is 3×10 4 ~1.2×10 5 .

3. A method for synthesizing a polyamide-imide containing a furan ring structure as claimed in any one of claims 1 to 2, characterized in that: The following steps are involved: 1) contacting an aromatic diamine containing a furan ring structure, an aromatic tetracarboxylic acid, a first catalyst and water to carry out a polycondensation reaction to obtain an aqueous suspension, and dehydrating and drying the aqueous suspension to obtain a polyamic acid containing a furan ring structure; 2) subjecting the polyamic acid to a solid phase viscosity-increasing reaction and high-temperature imidization to obtain the polyamide-imide containing a furan ring structure.

4. The synthesis method according to claim 3, characterized in that The structural formula of the aromatic diamine containing a furan ring structure is shown in Formula II: Formula II; And / or, the aromatic tetracarboxylic acid is selected from one or more of pyromellitic acid, biphenyltetracarboxylic acid, 3,3',4,4'-dibenzophenonetetracarboxylic acid and 4,4-oxydiphthalic acid.

5. The synthesis method according to claim 4, characterized in that In step 1), the water content is 80-90% based on the total weight of the aromatic diamine containing a furan ring structure, the aromatic tetracarboxylic acid and water; and / or, the molar ratio of the aromatic diamine to the aromatic tetracarboxylic acid is 1.01-1.05:1; And / or, based on the total weight of the aromatic diamine containing a furan ring structure, the aromatic tetracarboxylic acid and water, the amount of the first catalyst added is 0.2-1.5 wt‰; and / or, the first catalyst is a hypophosphite catalyst; And / or, in step 1), the polycondensation reaction includes a first stage and a second stage.

6. The synthesis method according to claim 5, characterized in that The hypophosphite catalyst is selected from one or more of sodium hypophosphite, potassium hypophosphite, calcium hypophosphite, and magnesium hypophosphite; And / or, the first stage reaction temperature is 100-150°C; the first stage reaction time is 3-6h; And / or, the second stage reaction temperature is 130-180°C; the second stage reaction time is 3-6h; And / or, the pressure of the second stage reaction is 0.5~1.5MPa.

7. The synthesis method according to claim 4, characterized in that In step 1), the polycondensation reaction is also stirred, and the stirring rate is 50-400 r / min; and / or, carrying out the polycondensation reaction in an inert gas environment; And / or, using a centrifugal separator to carry out the dehydration and drying; And / or, the polycondensation reaction is carried out in a high-pressure polymerization reactor.

8. The synthesis method according to claim 6, characterized in that In step 2), the temperature of the solid phase viscosity enhancement reaction is 200-260°C; And / or, in step 2), the solid phase viscosity enhancement reaction time is 4 to 10 hours; And / or, in step 2), the solid phase viscosity increasing reaction is carried out under vacuum conditions, wherein the vacuum degree of the vacuum conditions is 40-80 Pa; And / or, in step 2), a second catalyst is added during the solid phase viscosity increasing reaction, wherein the second catalyst is selected from one or more of diisopropylamine, 4-dimethylaminopyridine and triphenylphosphine; And / or, in step 2), a vacuum drum reactor is used to carry out the solid phase viscosity increasing reaction.

9. Use of the polyamide-imide containing a furan ring structure as claimed in any one of claims 1 to 2 in the preparation of a low dielectric film or in the preparation of an electronic product substrate or as an insulating material.

10. A low dielectric film, characterized in that: The method is prepared by using the polyamide-imide containing a furan ring structure as described in any one of claims 1 to 2.

Citation Information

Patent Citations

  • Polyimide resin containing furan ring and preparation method of polyimide resin

    CN108219133A

  • Furan ring-containing crosslinked polyimide resin and preparation method thereof

    CN108752928A

  • Furan ring-containing temperature-resistant polyimide resin and preparation method thereof

    CN112094410A

  • Bio-based fluorine-containing polyimide resin, preparation method thereof and polyimide film

    CN112321828A

  • Polyimide binder, preparation method thereof and silicon-carbon negative plate

    CN113429927A