Photo-curable polysiloxane, preparation method thereof and application of photo-curable polysiloxane as polymer solid electrolyte

By using photocurable high-dielectric constant polysiloxane in lithium-ion batteries, the problems of low ion conductivity and poor interfacial compatibility of solid polymer electrolyte membranes at room temperature are solved, and high dielectric constant and electrical are achieved The improvement of the chemical stability window has enhanced the safety and adaptability of lithium-ion batteries.

CN118994586AActive Publication Date: 2024-11-22INST OF CHEM CHINESE ACAD OF SCI
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310557557.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-17
Publication Date
2024-11-22
Estimated Expiration
2043-05-17

AI Technical Summary

Technical Problem

The existing solid polymer electrolyte membrane has low ionic conductivity at room temperature and poor interface compatibility with the electrode, which limits the application temperature range and safety of lithium-ion batteries.

Method used

Using photocurable high dielectric constant polysiloxane, it is prepared by introducing special polar side chains and photocurable acrylate groups into the polymer, and blended with lithium salts in situ. UV curing, a solid electrolyte membrane with high dielectric constant was prepared, which improved the ionic conductivity and interface compatibility of the membrane.

Benefits of technology

The room temperature ionic conductivity and electrochemical stability window of solid polymer electrolyte membrane are significantly improved, and the safety performance of lithium-ion batteries and their ability to adapt to high-temperature environments are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994586A_ABST
    Figure CN118994586A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of photocurable polysiloxane with a high dielectric constant and application of a solid electrolyte membrane containing the elastomer. The polysiloxane with the high dielectric constant is polysiloxane with a side chain containing a special polar group and a chain end containing a photocurable acrylate group or epoxy group, and the polysiloxane with the high dielectric constant is prepared through ring-opening polymerization reaction of a ring body containing the special polar side chain. And blending with a lithium salt, coating the surface of a pole piece with the mixture, and performing in-situ ultraviolet irradiation curing to obtain the electrolyte membrane. The preparation process of the polymer is simple, the ionic conductivity of the solid polymer electrolyte membrane can be effectively controlled according to needs, meanwhile, the interfacial compatibility of the solid polymer electrolyte membrane and a pole piece is improved through an in-situ curing method, the interface impedance between the solid polymer electrolyte membrane and the pole piece can be further reduced, and the performance of the solid polymer electrolyte membrane is improved. And the practical application of the polysiloxane-based solid polymer electrolyte membrane is promoted. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of polymer preparation and solid polymer electrolyte for lithium ion battery, and relates to a preparation method of a photocurable high dielectric constant polysiloxane, and the application of a solid electrolyte membrane containing the elastomer. Specifically, a polysiloxane-based solid electrolyte membrane with high ion transmission performance is prepared by mixing a high dielectric constant polysiloxane and a lithium salt and then photocuring, and the membrane is applied to lithium ion batteries. Background Art

[0002] Lithium-ion batteries have the advantages of high energy density, long cycle life, high output power and no memory effect. They are widely used in portable electronic products and electric vehicles. Lithium-ion batteries are composed of positive electrodes, negative electrodes, separators and electrolytes. The electrolyte is usually a flammable organic electrolyte, mainly including low-boiling point carbonates, ethers and hydroxy acid esters organic solvents, which pose a huge risk of being flammable and explosive. New solid electrolytes can replace the separators and electrolyte components in traditional lithium-ion batteries, which is expected to fundamentally solve the problem of safe use of batteries and further expand the temperature range of battery use. It is one of the most concerned research directions in recent years. Solid electrolytes are divided into inorganic solid electrolytes and solid polymer electrolytes. The lithium ion migration number of inorganic solid electrolytes is close to 1, and the room temperature ionic conductivity can reach 10 -2 S / cm, but its preparation process is complicated and the interface problem is serious. There are still many problems to be solved before application. In comparison, solid polymer electrolytes have the characteristics of high energy density, good safety, high interface compatibility and good flexibility, wider working range, easier to mass produce, and gradually become the development trend and research hotspot of the new generation of electrolytes.

[0003] The transmission of lithium ions in solid polymer electrolyte membranes follows the amorphous region conduction mechanism. Under the action of electric field force, lithium ions form coordination structures with polar groups, and the complexation-decomplexation process continues to occur with the thermal motion of polymer segments, completing directional migration. Therefore, the polymer matrix must contain polar groups that can produce ion-dipole interactions with lithium ions. According to the type of polymer groups, solid polymer electrolyte membranes are mainly divided into polyethers, polycarbonates, polyacrylonitrile and polyvinylidene fluoride. However, the glass transition temperatures of these polar polymer matrices are generally above room temperature, and even obvious crystallization phenomena will occur, resulting in limited low-temperature segment mobility and can only be used in high-temperature environments. Therefore, it is urgent to develop a polymer system that still has good segment mobility at room temperature in order to improve the room temperature ionic conductivity of solid polymer electrolyte membranes. Polysiloxane, as an organic-inorganic hybrid polymer, has a low glass transition temperature (Tg≈-123℃) and excellent segment mobility. It has great application prospects when used as a matrix for low-temperature electrolyte membranes. However, the intrinsic ionic conductivity of the commonly used methyl-substituted polysiloxane system is only 10 -10 S cm -1 In order to enable polysiloxane to be used as a matrix for solid polymer electrolyte membranes and to move from the laboratory to commercial applications, its ionic conductivity, stability and interfacial compatibility with electrodes need further research and improvement. Summary of the invention

[0004] In order to improve the above technical problems, the present invention provides a method for preparing a photocurable high dielectric constant polysiloxane and the application of a solid electrolyte membrane containing the elastomer. The high dielectric constant polysiloxane of the present invention is a polysiloxane having a special polar group in the side chain and a photocurable acrylate group or epoxy group at the chain end. The high dielectric constant polysiloxane is prepared by a ring-opening polymerization reaction of a ring body containing a special polar side chain. After being blended with a lithium salt, it is coated on the surface of the pole piece and cured by in-situ ultraviolet light to obtain an electrolyte membrane. The preparation process of the polymer in the present invention is simple, and the ionic conductivity of the solid polymer electrolyte membrane can be effectively controlled as needed. At the same time, the in-situ curing method increases the interface compatibility between the solid polymer electrolyte membrane and the pole piece, which can further reduce the interface impedance between the two, and promote the practical application of polysiloxane-based solid polymer electrolyte membranes.

[0005] The present invention is achieved through the following technical solutions:

[0006] A photocurable high dielectric constant polysiloxane comprising at least one polymer having a structure shown in formula I;

[0007]

[0008] Wherein, R1, R2 and R3 are the same or different and are independently selected from C 1-6 Alkyl, C 6-12 Aryl substituted C 1-6 Alkyl, C 6-12 Aryl, at least one C 1-6 Alkyl substituted C 6-12 Aryl;

[0009] R4 is selected from CN, CHO, nitro, amino, COOH, halogen or C 1-6 alkyl, provided that the C 1-6 The alkyl group is substituted by one, two or more of the following groups: CN, CHO, nitro, amino, COOH or halogen;

[0010] Each R5 is the same or different and is independently selected from C 1-6 Alkyl, C 6-12 Aryl substituted C 1-6 Alkyl, C 6-12 Aryl, at least one C 1-6 Alkyl substituted C 6-12 Aryl, -C 1-6 Alkyl-acrylate, -C 1-6 Alkyl-methacrylate or -OC 1-6 Alkyl-C 2-4 Epoxyalkyl; provided that at least one of the R5 at both ends of the polymer in Formula Ⅰ is selected from one of the following groups: -C 1-6 Alkyl-acrylate, -C 1-6 Alkyl-methacrylate or -OC 1-6 Alkyl-C 2-4 Epoxyalkyl;

[0011] m+n is any integer greater than 0 and less than or equal to 1000, and m is not 0.

[0012] According to an embodiment of the present invention, R1, R2 and R3 are the same or different and are each independently selected from methyl, ethyl, ethylphenyl, 2,4-dimethylphenyl or benzyl.

[0013] According to an embodiment of the present invention, R4 is selected from nitro, amino, -CH2X, -CH(X)CH3, -CH2CH2X, -CY3, -CH(Y)CH(Y)2, -C(Y)2CH2Y, wherein X is selected from -CN, amino, -C(=O)H, -COOH or halogen, and Y is selected from halogen; specifically, the halogen is selected from F, Cl, Br or I, and further specifically, selected from F or Cl; illustratively, X is selected from -CN, amino or Cl, and Y is selected from F.

[0014] According to an embodiment of the present invention, each R5 is the same or different and is independently selected from methyl, ethyl, -(CH2)3OC(=O)C(CH3)=CH2, -(CH2)3OC(=O)CH=CH2 or -OCH2(CHCH2O), provided that at least one of the R5 at both ends of the polymer in Formula I is -(CH2)3OC(=O)C(CH3)=CH2, -(CH2)3OC(=O)CH=CH2 or -OCH2(CHCH2O).

[0015] According to an embodiment of the present invention, m is any integer within the range of 1 to 1000, and n is any integer within the range of 0 to 999. Preferably, m is any integer within the range of 100 to 500, and n is any integer within the range of 0 to 499.

[0016] In a specific embodiment of the present invention, the polymer having the structure shown in formula I may have a structure shown in any one of the following formulas Ⅰ-A, Ⅰ-B, Ⅰ-C, Ⅰ-D, Ⅰ-E, and Ⅰ-F:

[0017]

[0018]

[0019] In formulas Ⅰ-A, Ⅰ-B, Ⅰ-C, Ⅰ-D, Ⅰ-E and IF, m and n have the same meanings as above.

[0020] In a specific embodiment of the present invention, in Formula Ⅰ-A, m may specifically be 100, and n may specifically be 400; in Formula Ⅰ-A, m may specifically be 200, and n may specifically be 300; in Formula Ⅰ-A, m may specifically be 300, and n may specifically be 200; in Formula Ⅰ-A, m may specifically be 400, and n may specifically be 100; in Formula Ⅰ-A, m may specifically be 450, and n may specifically be 50; in Formula Ⅰ-A, m may specifically be 500, and n may specifically be 0; m may specifically be 103, and n may specifically be 309; m may specifically be 198, and n may specifically be 198; m may specifically be 297, and n may specifically be 99; m may specifically be 404, and n may specifically be 0.

[0021] In a specific embodiment of the present invention, in Formula I-B, m may specifically be 100, and n may specifically be 400; in Formula I-B, m may specifically be 200, and n may specifically be 300; in Formula I-B, m may specifically be 300, and n may specifically be 200; in Formula I-B, m may specifically be 400, and n may specifically be 100; in Formula I-B, m may specifically be 450, and n may specifically be 50; in Formula I-B, m may specifically be 500, and n may specifically be 0; m may specifically be 404, and n may specifically be 0.

[0022] In a specific embodiment of the present invention, in Formula Ⅰ-C, m may specifically be 100, and n may specifically be 400; in Formula Ⅰ-C, m may specifically be 200, and n may specifically be 300; in Formula Ⅰ-C, m may specifically be 300, and n may specifically be 200; in Formula Ⅰ-C, m may specifically be 400, and n may specifically be 100; in Formula Ⅰ-C, m may specifically be 450, and n may specifically be 50; in Formula Ⅰ-C, m may specifically be 500, and n may specifically be 0.

[0023] In a specific embodiment of the present invention, in Formula Ⅰ-D, m may specifically be 100, and n may specifically be 400; in Formula Ⅰ-D, m may specifically be 200, and n may specifically be 300; in Formula Ⅰ-D, m may specifically be 300, and n may specifically be 200; in Formula Ⅰ-D, m may specifically be 400, and n may specifically be 100; in Formula Ⅰ-D, m may specifically be 450, and n may specifically be 50; in Formula Ⅰ-D, m may specifically be 500, and n may specifically be 0.

[0024] In a specific embodiment of the present invention, in Formulas Ⅰ-E and IF, m may specifically be 100, and n may specifically be 400; in Formula Ⅰ-E, m may specifically be 200, and n may specifically be 300; in Formula Ⅰ-E, m may specifically be 300, and n may specifically be 200; in Formula Ⅰ-E, m may specifically be 400, and n may specifically be 100; in Formula Ⅰ-E, m may specifically be 450, and n may specifically be 50; in Formula Ⅰ-E, m may specifically be 500, and n may specifically be 0; in Formula Ⅰ-F, m may specifically be 404, and n may specifically be 0.

[0025] According to an embodiment of the present invention, the dielectric constant of the polysiloxane is 2-20 (10 5 Hz), preferably with a dielectric constant of 8.5-18.5 (10 5 Hz).

[0026] The present invention further provides a method for preparing the above-mentioned photocurable high dielectric constant polysiloxane, comprising the following steps: using a cyclosiloxane monomer having a polar side chain substitution having a structure shown in Formula II and a compound having a structure shown in Formula III as a capping agent to carry out a ring-opening polymerization reaction under the action of a catalyst to obtain a polysiloxane shown in Formula I;

[0027]

[0028] In Formula II, a+b is any integer greater than 2 and less than or equal to 6, and a is not 0; R1, R2, R3, and R4 have the above meanings;

[0029]

[0030] In formula III, R5 has the same meaning as above.

[0031] According to an embodiment of the present invention, the molar ratio of the polymer having the structure represented by Formula II to the compound having the structure represented by Formula III may be 250:(15-1), specifically 250:(10-2), for example, 250:10, 250:9, 250:8, 250:7, 250:6, 250:5, 250:4, 250:3, 250:2 or 250:1.

[0032] According to an embodiment of the present invention, the ring-opening polymerization reaction is carried out in an organic solvent.

[0033] According to an embodiment of the present invention, the organic solvent may be one or more of N-methylpyrrolidone, N,N-dimethylformamide, 1,4-dioxane, ethyl acetate, chloroform, tetrahydrofuran, toluene, methanol, ethanol, isopropanol, butanol, hexane, benzene, acetone, butanone, cyclohexanone, o-xylene, p-xylene and m-xylene.

[0034] According to an embodiment of the present invention, the mass of the organic solvent may be 0.5 to 10 times the total mass of the polymer having the structure shown in Formula II and the compound having the structure shown in Formula III, specifically 1 to 5 times, for example, 1 time, 2 times, 3 times, 4 times, 5 times or 6 times.

[0035] According to an embodiment of the present invention, the catalyst may be an anionic catalyst or a cationic catalyst.

[0036] According to an embodiment of the present invention, the anion catalyst may be one or more of KOH, NaOH, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrabutylphosphonium hydroxide, benzyltrimethylammonium bis(catechol)phenylsiliconate, n-butyl lithium, potassium tert-butoxide, lithium hydroxide, diethylamine, lithium siliconate, and potassium siliconate.

[0037] According to an embodiment of the present invention, the cationic catalyst may be one or more of concentrated H2SO4, HClO4, Lewis acid, trifluoromethylsulfonic acid, and bis(trifluoromethylsulfonyl)imide.

[0038] According to an embodiment of the present invention, the mass of the catalyst may be 0.05% to 20% of the total mass of the polymer having the structure shown in Formula II and the compound having the structure shown in Formula III, specifically 0.1% to 10%, for example 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7% or 8%.

[0039] According to an embodiment of the present invention, the temperature of the ring-opening polymerization reaction may be 25°C to 130°C, specifically 35°C to 120°C, for example 35°C, 50°C, 70°C, 80°C, 95°C or 110°C.

[0040] According to an embodiment of the present invention, the ring-opening polymerization reaction time may be 0.1 h to 48 h, specifically 0.3 h to 24 h, for example 0.5 h, 2 h, 4 h, 6 h, 8 h, 12 h or 24 h.

[0041] According to an embodiment of the present invention, the preparation method comprises the following specific steps:

[0042] Step 1: Mix the compounds having the structures shown in Formula II and Formula III in an organic solvent under continuous mechanical stirring;

[0043] Step 2: Under the protection of an inert atmosphere (such as N2), add an appropriate amount of catalyst, raise the temperature to the desired reaction temperature, continue to stir the reaction, and use silicon spectrum to confirm whether the reaction has reached equilibrium. After the reaction is completed, the photocurable high dielectric constant polysiloxane can be obtained.

[0044] In some embodiments of the present invention, the polymer having the structure shown in Formula II may specifically be a cyclosiloxane monomer containing polar side chain substitution having the structures shown in the following Formula II-A, Formula II-B, and Formula II-C:

[0045]

[0046] In Formula II-A and Formula II-B, a+b can specifically be 4, and a is not equal to 0, for example, a is 1 and b is 3; a is 2 and b is 2; a is 3 and b is 1 or a is 4 and b is 0.

[0047] In formula II-C, a+b can specifically be 3, and a is not equal to 0, for example, a is 1 and b is 2; a is 2 and b is 1; a is 3 and b is 0.

[0048] In some embodiments of the present invention, the compound having the structure shown in Formula III may specifically be a compound having the structure shown in the following Formula III-A:

[0049]

[0050] The present invention also provides the use of the photocurable high dielectric constant polysiloxane in the preparation of solid polymer electrolyte membrane materials for lithium ion batteries.

[0051] The solid polymer electrolyte material for lithium ion batteries of the present invention comprises: the photocurable high dielectric constant polysiloxane as described above, a lithium salt and a photoinitiator.

[0052] According to an embodiment of the present invention, the solid polymer electrolyte material for lithium ion battery is prepared by the following method:

[0053] Step 1: Add the above polysiloxane and lithium salt into a light-proof reaction bottle, and fully dissolve and mix the two in an organic solvent to obtain a uniform colorless and transparent solution;

[0054] Step 2: Add photoinitiator to the above mixed solution, stir evenly and pour the solution into a polytetrafluoroethylene mold, dry it in a vacuum oven at 30-60°C for 24-48 hours, then place it in a glove box and cure it under ultraviolet light to obtain a solid polymer electrolyte membrane material with a film thickness of 200-400μm.

[0055] According to the present invention, the lithium salt in step 1 can be LiNO3, LiClO4, LiBF4, LiAsF6, LiPF6, LiBOB, LiDFOB, LiFSI, LiTFSI, LiSbF6, LiN(C4F9SO2)2, LiCF3CO2, LiAlCl4, Li2B 12 F 12 , LiCF3SO3 or more.

[0056] According to the present invention, the mass percentage of the lithium salt in step 1 can be 10% to 400% of the polysiloxane, for example, 30% to 200%, such as 10%, 30%, 50%, 70%, 100%, 130%, 150% or 200%.

[0057] According to the present invention, the organic solvent in step 1 can be one or more of N-methylpyrrolidone, N,N-dimethylformamide, 1,4-dioxane, ethyl acetate, chloroform, tetrahydrofuran, toluene, methanol, ethanol, isopropanol, butanol, hexane, benzene, acetone, butanone, cyclohexanone, o-xylene, p-xylene and m-xylene.

[0058] According to the present invention, the mass of the organic solvent in step 1 may be 2 to 10 times the total mass of the polysiloxane and the lithium salt, specifically 2 to 6 times, for example 2 times, 3 times, 4 times, 5 times or 6 times.

[0059] According to the present invention, the photoinitiator in step 2 may be one or more of 2,4,6 (trimethylbenzoyl) diphenylphosphine oxide (TPO photoinitiator), ethyl 2,4,6-trimethylbenzoylphosphonate (TPO-L photoinitiator), 2-methyl-1-[4-methylthiophenyl]-2-morpholinyl-1-propanone (907 photoinitiator), 2-isopropylthioxanthone (2,4 isomer mixture) (ITX photoinitiator), 4-dimethylamino-ethyl benzoate (EDB photoinitiator), 1-hydroxy-cyclohexyl phenyl ketone (184 photoinitiator), 2-hydroxy-2-methyl-1-phenyl-1-propanone (1173 photoinitiator), 2,2-dimethoxy-2-phenylethanone (BDK photoinitiator) or methyl o-benzoylbenzoate (0MBB photoinitiator).

[0060] According to the present invention, the mass percentage of the photoinitiator in step 2 can be 0.05% to 10% of the polysiloxane, specifically 0.5% to 5%, for example 0.5%, 1%, 2%, 3%, 4% or 5%.

[0061] According to the present invention, the ultraviolet light irradiation time in step 2 can be 0.1h to 6h, specifically 0.2h to 2h, for example 0.2h, 0.4h, 0.6h, 0.8h, 1h, 1.5h or 2h.

[0062] According to the present invention, the wavelength of the ultraviolet lamp in step 2 may be 200-400 nm, specifically 220-400 nm, for example 231 nm, 244 nm, 253 nm, 258 nm, 273 nm, 299 nm, 307 nm, 365 nm or 370 nm.

[0063] According to the present invention, the film thickness of the solid polymer electrolyte membrane material is 200nm-400nm, preferably 250nm.

[0064] According to the present invention, the room temperature ionic conductivity of the solid polymer electrolyte membrane material is 1×10 -6 ~8×10 -5 S cm -1 .

[0065] According to the present invention, the high temperature (80°C) ionic conductivity of the solid polymer electrolyte membrane material is 1×10 -4 ~8×10 -3 Scm -1 .

[0066] According to the present invention, the room temperature electrochemical stability window of the solid polymer electrolyte membrane material is 1×5.2~5.6V (vs Li / Li + ).

[0067] Beneficial effects of the present invention:

[0068] Compared with the prior art, the photocurable high dielectric constant polysiloxane of the present invention has high thermal stability, a glass transition temperature far below room temperature, and greatly shortens the curing time compared to the thermal curing method of silicone elastomers. The preparation process is simple and has good compatibility with lithium salts.

[0069] The solid polymer electrolyte membrane material prepared using the above-mentioned high dielectric constant polysiloxane has good flexibility, high ionic conductivity, wide electrochemical stability window, high heat resistance, and can be adapted for use with high-voltage positive electrode materials; based on the use of the polysiloxane matrix, the solid polymer electrolyte membrane material of the present invention is green and environmentally friendly, has good thermal stability, is non-flammable, and has no leakage, which greatly improves the safety performance of lithium-ion batteries.

[0070] Definitions and explanations of terms

[0071] In this document, the terms “include”, “comprises” and / or “contains” are open expressions, that is, they include the contents specified in the present invention but do not exclude other contents.

[0072] In this article, the term "any integer between 1 and 1000" means every integer between 1, 2, 3, 4, 5, 6, ... 1000. Due to space reasons, not all of them are listed here, but those skilled in the art will know that it includes every integer between 1 and 1000. In addition, the same definition also includes "any integer between 0 and 999", "any integer between 100 and 500", etc.

[0073] In this article, the term "halogen" means fluorine, chlorine, bromine and / or iodine. Accordingly, the term "halo" refers to fluoro, chloro, bromo and / or iodo. Within the scope of this article, when an atom, residue, group or part is halogenated, the atom in the halogenated position can be monosubstituted, disubstituted or polysubstituted by a halogen atom up to full substitution.

[0074] The term "C 1-6 “Alkyl” is understood as meaning a linear or branched, saturated, monovalent hydrocarbon radical having 1, 2, 3, 4, 5 or 6 carbon atoms. The alkyl radical is, for example, methyl, ethyl, propyl, butyl, pentyl, hexyl, isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, 2-methylbutyl, 1-methylbutyl, 1-ethylpropyl, 1,2-dimethylpropyl, neopentyl, 1,1-dimethylpropyl, 4-methylpentyl, 3-methylpentyl, 2-methylpentyl, 1-methylpentyl, 2-ethylbutyl, 1-ethylbutyl, 3,3-dimethylbutyl, 2,2-dimethylbutyl, 1,1-dimethylbutyl, 2,3-dimethylbutyl, 1,3-dimethylbutyl or 1,2-dimethylbutyl, etc. or their isomers. In particular, the radical has 1, 2 or 3 carbon atoms (“C 1-3 alkyl"), for example methyl, ethyl, n-propyl or isopropyl.

[0075] The term "C 2-4 "Oxiranyl" means a saturated monovalent monocyclic hydrocarbon ring containing 1 or 2 O atoms and 2 to 4 carbon atoms. 2-4 Examples of the alkylene oxide group include, but are not limited to, ethylene oxide, propylene oxide or butylene oxide.

[0076] The term "C 6-12 "Aryl" is understood to mean a monovalent aromatic or partially aromatic monocyclic, bicyclic or tricyclic hydrocarbon ring ("C 6-12or a ring having 9 carbon atoms ("C9 aryl"), for example indanyl or indenyl, or a ring having 10 carbon atoms ("C 10 "aryl"), for example tetrahydronaphthyl, dihydronaphthyl or naphthyl.

[0077] The above term “C 1-6 The definition of "alkyl" also applies to compounds containing "C 1-6 Other terms for "alkyl", such as the term "halo-C 1-6 alkyl". BRIEF DESCRIPTION OF THE DRAWINGS

[0078] Figure 1 The H-NMR spectra of the photocurable high dielectric constant polysiloxanes of Examples 1-4 and the photocurable polysiloxane control sample of Comparative Example 1 are shown.

[0079] Figure 2 This is the gel permeation chromatogram of the photocurable high dielectric constant polysiloxane of Example 4. Figure 3 The infrared spectra of the photocurable high dielectric constant polysiloxanes of Examples 1-4 and the photocurable polysiloxane control sample of Comparative Example 1 are shown.

[0080] Figure 4 The DSC spectra of the photocurable high dielectric constant polysiloxanes of Examples 1-4 and the photocurable polysiloxane control sample of Comparative Example 1 are shown.

[0081] Figure 5 This is the surface morphology of the solid polymer electrolyte membrane material of Example 8.

[0082] Figure 6 This is the cross-sectional morphology of the solid polymer electrolyte membrane material of Example 8.

[0083] Figure 7 The AC impedance spectra of the solid polymer electrolyte membrane material of Example 4 at different temperatures.

[0084] Figure 8 This is the electrochemical stability window of the solid polymer electrolyte membrane material of Example 4 tested at room temperature.

[0085] Fig. 9 This is a bending picture of the solid polymer electrolyte membrane material of Example 8.

[0086] Fig.10 This is the thermal gravimetric curve of the solid polymer electrolyte membrane material of Example 8. DETAILED DESCRIPTION

[0087] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.

[0088] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.

[0089] The test and calculation method of ionic conductivity (σ) in the following examples is as follows: the solid electrolyte membrane material is sandwiched between two stainless steel electrodes (SS) to assemble into SS / SPE / SS blocking electrodes for ionic conductivity testing. The AC impedance spectrum of the blocking cell is obtained on an electrochemical workstation, and the bulk impedance Rs of the electrolyte is recorded. The frequency range of the test is 10 6 -10 -1 Hz, and the disturbance voltage is 10mV. The ionic conductivity (σ) of the electrolyte is calculated by the following formula:

[0090]

[0091] Where, l (cm) is the thickness of the electrolyte membrane; Rs (Ω) is the bulk impedance of the electrolyte membrane; S (cm 2 ) is the contact area between the electrolyte membrane and the stainless steel electrode. It was sandwiched between the stainless steel electrode (SS) and the lithium metal electrode (Li) to assemble a Li / SPE / SS test cell, and the electrochemical stability of the electrolyte was tested by linear sweep voltammetry (LSV). The potential range of the LSV test was 0-6.5 V, and the scan rate was 1 mV s -1 .

[0092] The electrochemical properties of the materials in the following examples and comparative examples were tested at a certain temperature using an Autolab 302N electrochemical workstation produced by Swiss Metrohm and a CHI1600E electrochemical workstation produced by Shanghai Chenhua Instrument Co., Ltd.

[0093] Example 1: Preparation of photocurable high dielectric constant polysiloxane and solid polymer electrolyte membrane material

[0094] Preparation of photocurable high dielectric constant polysiloxane: Under N2 protection, 50g of methyl cyanopropyl cyclosiloxane (Formula II-A) and 0.5g of (1,1,3,3-tetramethyldisiloxane-1,3-diyl) dipropane-1,3-diyl diacrylate (Formula III-A) were added to a 500ml three-necked flask, and 100g of N,N-dimethylformamide was added at the same time, and stirred for 10 minutes until the system was uniform. The temperature was raised to 70°C, and 1g of concentrated H2SO4 was pipetted into the above three-necked flask with a pipette. After reacting for 48 hours, the solvent and catalyst were removed to obtain the polymer shown in Ⅰ-A (where m is 103; n is 309), which is a photocurable high dielectric constant polysiloxane named PCDMS-1.

[0095] In the structure represented by formula II-A, a is 1 and b is 3.

[0096] Preparation of solid polymer electrolyte membrane material: In a glove box (H2O < 0.1ppm, O2 < 0.1ppm), 1.0g PCDMS-1, 0.45g LiTFSI and 0.02g BDK photoinitiator were fully dissolved in 4g N,N-dimethylformamide to form a uniform, transparent, colorless solution. The solution was cast on a tetrafluoroethylene mold, and after the organic solvent was volatilized in a vacuum oven, it was irradiated with 360nm ultraviolet light in the glove box for 2h until it was completely cured, and a solid polymer electrolyte membrane material was obtained, named SPE-1.

[0097] The dielectric constant of the photocurable high dielectric constant polysiloxane prepared in this example is shown in Table 1.

[0098] The electrochemical properties of the solid polymer electrolyte membrane material prepared in this example are shown in Table 2 and Table 3.

[0099] Example 2: Preparation of photocurable high dielectric constant polysiloxane and solid polymer electrolyte membrane material

[0100] Preparation of photocurable high dielectric constant polysiloxane: Under N2 protection, 50g of methyl cyanopropyl cyclosiloxane (Formula II-A) and 0.45g of (1,1,3,3-tetramethyldisiloxane-1,3-diyl) dipropane-1,3-diyl diacrylate (Formula III-A) were added to a 500ml three-necked flask, and 100g of N,N-dimethylformamide was added at the same time, and stirred for 10 minutes until the system was uniform. The temperature was raised to 70°C, and 1g of concentrated H2SO4 was pipetted into the above three-necked flask with a pipette. After reacting for 48 hours, the solvent and catalyst were removed to obtain the polymer shown in Ⅰ-A (where m is 198; n is 198), that is, a photocurable high dielectric constant polysiloxane named PCDMS-2.

[0101] In the structure represented by formula II-A, a is 2 and b is 2.

[0102] Preparation of solid polymer electrolyte membrane material: In a glove box (H2O<0.1ppm, O2<0.1ppm), 1.0g PCDMS-2, 0.45g LiTFSI and 0.02g BDK photoinitiator were fully dissolved in 4g N,N-dimethylformamide to form a uniform, transparent, colorless solution. The solution was cast on a tetrafluoroethylene mold, and after the organic solvent was volatilized in a vacuum oven, it was irradiated with 360nm ultraviolet light in the glove box for 2h until it was completely cured, and a solid polymer electrolyte membrane material was obtained, named SPE-2.

[0103] The dielectric constant of the photocurable high dielectric constant polysiloxane prepared in this example is shown in Table 1.

[0104] The electrochemical properties of the solid polymer electrolyte membrane material prepared in this example are shown in Table 2 and Table 3.

[0105] Example 3: Preparation of photocurable high dielectric constant polysiloxane and solid polymer electrolyte membrane material

[0106] Preparation of photocurable high dielectric constant polysiloxane: Under N2 protection, 50g of methyl cyanopropyl cyclosiloxane (Formula II-A) and 0.4g of (1,1,3,3-tetramethyldisiloxane-1,3-diyl) dipropane-1,3-diyl diacrylate (Formula III-A) were added to a 500ml three-necked flask, and 100g of N,N-dimethylformamide was added at the same time, and stirred for 10 minutes until the system was uniform. The temperature was raised to 70°C, and 1g of concentrated H2SO4 was pipetted into the above three-necked flask with a pipette. After reacting for 48 hours, the solvent and catalyst were removed to obtain the polymer shown in Ⅰ-A (where m is 297; n is 99), that is, a photocurable high dielectric constant polysiloxane named PCDMS-3.

[0107] In the structure represented by formula II-A, a is 3 and b is 1.

[0108] Preparation of solid polymer electrolyte membrane material: In a glove box (H2O < 0.1ppm, O2 < 0.1ppm), 1.0g PCDMS-3, 0.45g LiTFSI and 0.02g BDK photoinitiator were fully dissolved in 4g N,N-dimethylformamide to form a uniform, transparent, colorless solution. The solution was cast on a tetrafluoroethylene mold, and after the organic solvent was volatilized in a vacuum oven, it was irradiated with 360nm ultraviolet light in the glove box for 2h until it was completely cured, and a solid polymer electrolyte membrane material was obtained, named SPE-3.

[0109] The dielectric constant of the photocurable high dielectric constant polysiloxane prepared in this example is shown in Table 1.

[0110] The electrochemical properties of the solid polymer electrolyte membrane material prepared in this example are shown in Table 2 and Table 3.

[0111] Example 4: Preparation of photocurable high dielectric constant polysiloxane and solid polymer electrolyte membrane material

[0112] Preparation of photocurable high dielectric constant polysiloxane: Under N2 protection, 50g of methyl cyanopropyl cyclosiloxane (Formula II-A) and 0.35g of (1,1,3,3-tetramethyldisiloxane-1,3-diyl) dipropane-1,3-diyl diacrylate (Formula III-A) were added to a 500ml three-necked flask, and 100g of N,N-dimethylformamide was added at the same time, and stirred for 10 minutes until the system was uniform. The temperature was raised to 70°C, and 1g of concentrated H2SO4 was pipetted into the above three-necked flask with a pipette. After reacting for 48 hours, the solvent and catalyst were removed to obtain the polymer shown in Ⅰ-A (where m is 404; n is 0), that is, a photocurable high dielectric constant polysiloxane named PCMS-4.

[0113] In the polymer represented by formula II-A, a is 4 and b is 0.

[0114] Preparation of solid polymer electrolyte membrane material: In a glove box (H2O < 0.1ppm, O2 < 0.1ppm), 1.0g PCMS-4, 0.45g LiTFSI and 0.02g BDK photoinitiator were fully dissolved in 4g N,N-dimethylformamide to form a uniform, transparent, colorless solution. The solution was cast on a tetrafluoroethylene mold, and after the organic solvent was volatilized in a vacuum oven, it was irradiated with 360nm ultraviolet light in the glove box for 2h until it was completely cured, and a solid polymer electrolyte membrane material was obtained, named SPE-4.

[0115] The dielectric constant of the photocurable high dielectric constant polysiloxane prepared in this example is shown in Table 1.

[0116] The electrochemical properties of the solid polymer electrolyte membrane material prepared in this example are shown in Table 2 and Table 3.

[0117] Example 5: Preparation of photocurable high dielectric constant polysiloxane and solid polymer electrolyte membrane material

[0118] Preparation of photocurable high dielectric constant polysiloxane: The preparation process is the same as Example 4.

[0119] Preparation of solid polymer electrolyte membrane material: In a glove box (H2O<0.1ppm, O2<0.1ppm), 1.0g PCMS-4, 0.75g LiTFSI and 0.02g BDK photoinitiator were fully dissolved in 4g N,N-dimethylformamide to form a uniform, transparent, colorless solution. The solution was cast on a tetrafluoroethylene mold, and after the organic solvent was volatilized in a vacuum oven, it was irradiated with 360nm ultraviolet light in the glove box for 2h until it was completely cured, and a solid polymer electrolyte membrane material was obtained, named SPE-5.

[0120] The electrochemical properties of the solid polymer electrolyte membrane material prepared in this example are shown in Table 2 and Table 3.

[0121] Example 6: Preparation of photocurable high dielectric constant polysiloxane and solid polymer electrolyte membrane material

[0122] Preparation of photocurable high dielectric constant polysiloxane: The preparation process is the same as Example 4.

[0123] Preparation of solid polymer electrolyte membrane material: In a glove box (H2O<0.1ppm, O2<0.1ppm), 1.0g PCMS-4, 1.00g LiTFSI and 0.02g BDK photoinitiator were fully dissolved in 4g N,N-dimethylformamide to form a uniform, transparent, colorless solution. The solution was cast on a tetrafluoroethylene mold, and after the organic solvent was volatilized in a vacuum oven, it was irradiated with 360nm ultraviolet light in the glove box for 2h until it was completely cured, and a solid polymer electrolyte membrane material was obtained, named SPE-6.

[0124] The electrochemical properties of the solid polymer electrolyte membrane material prepared in this example are shown in Table 2 and Table 3.

[0125] Example 7: Preparation of photocurable high dielectric constant polysiloxane and solid polymer electrolyte membrane material

[0126] Preparation of photocurable high dielectric constant polysiloxane: The preparation process is the same as Example 4.

[0127] Preparation of solid polymer electrolyte membrane material: In a glove box (H2O < 0.1ppm, O2 < 0.1ppm), 1.0g PCMS-4, 1.30g LiTFSI and 0.02g EDK photoinitiator were fully dissolved in 4g N,N-dimethylformamide to form a uniform, transparent, colorless solution. The solution was cast on a tetrafluoroethylene mold, and after the organic solvent was volatilized in a vacuum oven, it was irradiated with 360nm ultraviolet light in the glove box for 2h until it was completely cured, and a solid polymer electrolyte membrane material was obtained, named SPE-7.

[0128] The electrochemical properties of the solid polymer electrolyte membrane material prepared in this example are shown in Table 2 and Table 3.

[0129] Example 8: Preparation of photocurable high dielectric constant polysiloxane and solid polymer electrolyte membrane material

[0130] Preparation of photocurable high dielectric constant polysiloxane: The preparation process is the same as Example 4.

[0131] Preparation of solid polymer electrolyte membrane material: In a glove box (H2O<0.1ppm, O2<0.1ppm), 1.0g PCMS-4, 1.50g LiTFSI and 0.02g BDK photoinitiator were fully dissolved in 4g N,N-dimethylformamide to form a uniform, transparent, colorless solution. The solution was cast on a tetrafluoroethylene mold, and after the organic solvent was volatilized in a vacuum oven, it was irradiated with 360nm ultraviolet light in the glove box for 2h until it was completely cured, and a solid polymer electrolyte membrane material was obtained, named SPE-8.

[0132] The electrochemical properties of the solid polymer electrolyte membrane material prepared in this example are shown in Table 2 and Table 3.

[0133] Example 9: Preparation of photocurable high dielectric constant polysiloxane and solid polymer electrolyte membrane material

[0134] Preparation of photocurable high dielectric constant polysiloxane: Under N2 protection, 50g of methylaminopropyl cyclosiloxane (Formula II-B) and 0.35g of (1,1,3,3-tetramethyldisiloxane-1,3-diyl)dipropane-1,3-diyl diacrylate (Formula III-A) were added to a 500ml three-necked flask, and 100g of N,N-dimethylformamide was added at the same time, and stirred for 10 minutes until the system was uniform. The temperature was raised to 70°C, and 1g of concentrated H2SO4 was pipetted into the above three-necked flask with a pipette. After reacting for 48 hours, the solvent and catalyst were removed to obtain the polymer shown in I-B (where m is 404; n is 0), that is, a photocurable high dielectric constant polysiloxane named PNMS.

[0135] In the polymer represented by formula II-B, a is 4 and b is 0.

[0136] Preparation of solid polymer electrolyte membrane material: In a glove box (H2O<0.1ppm, O2<0.1ppm), 1.0g PNMS, 0.45g LiTFSI and 0.02g BDK photoinitiator were fully dissolved in 4g N,N-dimethylformamide to form a uniform, transparent, colorless solution. The solution was cast on a tetrafluoroethylene mold, and after the organic solvent was volatilized in a vacuum oven, it was irradiated with 360nm ultraviolet light in the glove box for 2h until it was completely cured, and a solid polymer electrolyte membrane material was obtained, named SPE-9.

[0137] The dielectric constant of the photocurable high dielectric constant polysiloxane prepared in this example is shown in Table 1.

[0138] The electrochemical properties of the solid polymer electrolyte membrane material prepared in this example are shown in Table 2 and Table 3.

[0139] Example 10: Preparation of photocurable high dielectric constant polysiloxane and solid polymer electrolyte membrane material

[0140] Preparation of photocurable high dielectric constant polysiloxane: Under N2 protection, add 50g of trifluoropropylmethylcyclotrisiloxane (Formula II-C) and 0.35g of (1,1,3,3-tetramethyldisiloxane-1,3-diyl)dipropane-1,3-diyl diacrylate (Formula III-A) into a 500ml three-necked flask, and add 100g of N,N-dimethylformamide at the same time, and stir for 10 minutes until the system is uniform. Raise the temperature to 70°C, use a pipette to transfer 1g of concentrated H2SO4 into the above three-necked flask, react for 48h, remove the solvent and catalyst, and obtain the polymer shown in Ⅰ-F (where m is 404; n is 0), that is, a photocurable high dielectric constant polysiloxane named PFMS.

[0141] In the polymer represented by formula II-C, a is 4 and b is 0.

[0142] Preparation of solid polymer electrolyte membrane material: In a glove box (H2O<0.1ppm, O2<0.1ppm), 1.0g PFMS, 0.45g LiTFSI and 0.02g BDK photoinitiator were fully dissolved in 4g N,N-dimethylformamide to form a uniform, transparent, colorless solution. The solution was cast on a tetrafluoroethylene mold, and after the organic solvent was volatilized in a vacuum oven, it was irradiated with 360nm ultraviolet light in the glove box for 2h until it was completely cured, and a solid polymer electrolyte membrane material was obtained, named SPE-10.

[0143] The dielectric constant of the photocurable high dielectric constant polysiloxane prepared in this example is shown in Table 1.

[0144] The electrochemical properties of the solid polymer electrolyte membrane material prepared in this example are shown in Table 2 and Table 3.

[0145] Comparative Example 1: Preparation of photocurable polysiloxane control sample and solid polymer electrolyte membrane material

[0146] Preparation of photocurable polysiloxane control sample: Under N2 protection, add 50g of octamethylcyclotetrasiloxane (Formula II-A) and 0.6g of 1,3-bis(3-acryloxypropyl)tetramethyldisiloxane (Formula III-A) into a 500ml three-necked flask, and add 100g of N,N-dimethylformamide at the same time, and stir for 10 minutes until the system is uniform. Heat to 70°C, use a pipette to transfer 1g of concentrated H2SO4 into the above three-necked flask, react for 48h, remove the solvent and catalyst, and obtain the polymer shown in Ⅰ-A, that is, a photocurable polysiloxane (molecular weight of 30,000), named PDMS-0.

[0147] In the polymer represented by formula II-A, a is 0 and b is 4.

[0148] Preparation of solid polymer electrolyte membrane material: In a glove box (H2O<0.1ppm, O2<0.1ppm), 1.0g PDMS-0, 0.45g LiTFSI and 0.02g BDK photoinitiator were fully dissolved in 4g N,N-dimethylformamide to form a uniform, transparent, colorless solution. The solution was cast on a tetrafluoroethylene mold, and after the organic solvent was volatilized in a vacuum oven, it was irradiated with 360nm ultraviolet light in the glove box for 2h until it was completely cured, and a solid polymer electrolyte membrane material was obtained, named SPE-0.

[0149] The dielectric constant of the photocurable polysiloxane control sample prepared in this comparative example is shown in Table 1.

[0150] Comparative Example 2: Preparation of PEO-based solid polymer electrolyte membrane material

[0151] PEO-based solid polymer electrolyte membrane material: In a glove box (H2O < 0.1ppm, O2 < 0.1ppm), 1.0g PEO (molecular weight 600,000) and 0.45g LiTFSI were fully dissolved in 4g anhydrous acetonitrile to form a uniform, transparent, colorless solution. The solution was cast on a tetrafluoroethylene mold and dried in a vacuum oven at 80°C for 48h. After fully removing the organic solvent, a solid polymer electrolyte membrane material was obtained, named PEO SPE.

[0152] The electrochemical properties of the PEO-based solid polymer electrolyte membrane material prepared in this comparative example are shown in Tables 2 and 3.

[0153] Table 1 Dielectric constant data of photocurable polysiloxane in Examples 1-4 and Comparative Example 1

[0154]

[0155]

[0156] As can be seen from Table 1: the dielectric constant of the photocurable high dielectric constant polysiloxane prepared in the present application is significantly improved compared with the two comparative examples. Compared with comparative example 1, the dielectric constant of Example 4 is increased from 3.07 to 17.25. The increase in dielectric constant will help improve the polymer's ability to dissolve lithium salts, thereby increasing the number of carriers in the system. This result shows that the polysiloxane prepared in the present invention has excellent lithium salt dissociation ability.

[0157] Table 2 Ionic conductivity data of high dielectric silicone rubber in Examples 2-10 and Comparative Examples

[0158]

[0159]

[0160] Table 3. Electrochemical stability window data of high dielectric silicone rubber in Examples 2-10 and Comparative Examples

[0161] sample Stable potential range (V) Example 1 5.45 Example 2 5.57 Example 3 5.64 Example 4 5.23 Example 5 5.49 Example 6 5.54 Example 7 5.65 Example 8 5.74 Example 9 5.08 Example 10 5.68 Comparative Example 1 5.66 Comparative Example 2 4.32

[0162] It can be seen from Table 2 and Table 3 that the ionic conductivity of the solid polymer electrolyte membrane material prepared in the present application is significantly improved compared with the solid electrolyte based on PEO. For example, compared with Example 4 and Comparative Example 2, the conductivity at room temperature is increased from 5.2123×10 -6 S cm -1 Increased to 8.1873×10 -5 S cm -1 At the same time, due to the excellent chemical stability of the polysiloxane polymer itself, the electrochemical stability window of the solid polymer electrolyte membrane material prepared in this application is higher than 5V, which has higher electrochemical stability than the PEO system and is expected to be suitable for high-voltage battery systems.

[0163] Figure 1 The NMR hydrogen spectra of the photocurable high dielectric constant polysiloxane of Examples 1-4 and the photocurable polysiloxane control sample in Comparative Example 1. In Comparative Example 1, there is only a peak of Si-CH3 at 0.1ppm, and there are no other H structures in the system. In the spectra of Examples 1-4, there is a peak of Si-CH3 at 0.1ppm and a peak of Si- CH2 The peak corresponding to CH2CH2CN, 1.7ppm is Si-CH2 CH2The peak corresponding to CH2CN, 2.4ppm is Si-CH2CH2 CH2 Peak corresponding to CN. With the increase of polar group content, the peak intensity at 0.1ppm, 0.7ppm, 1.7ppm and 2.4ppm gradually increased, while the peak intensity at 0.1ppm gradually weakened.

[0164] Figure 2 This is a gel permeation chromatogram of the photocurable high dielectric constant polysiloxane of Example 4. The weight average molecular weight (Mw) of the prepared polymer is 104,900, and the number average molecular weight (Mn) is 31,600, which proves that the prepared polymer is a polymer.

[0165] Figure 3 The infrared spectra of the photocurable high dielectric constant polysiloxanes of Examples 1-4 and the photocurable polysiloxane control sample of Comparative Example 1 are shown in FIG. -1 , 1425cm -1 , 1346cm -1 The vibration peaks of -CH2(α), CH2(β), and CH2(γ) in -CH2(α)CH2(β)CH2(γ)CN are 1180 cm -1 The peaks near 1454cm -1 , 1425cm -1 , 1346cm -1 The peak intensity gradually increases.

[0166] Figure 4 The DSC spectra of the photocurable high dielectric constant polysiloxane of Examples 1-4 and the photocurable polysiloxane control sample in Comparative Example 1. Although Comparative Example 1 has a lower glass transition temperature (-123.65°C), it crystallizes at around -50°C, while the glass transition temperatures of the samples of Examples 1-4 increase with the increase of the polar group content, but are all below -60°C, and are all in a highly elastic state within the electrolyte use temperature range, with better performance.

[0167] Figure 5 This is the surface morphology of the solid polymer electrolyte membrane material of Example 8. It can be seen that the surface is flat and smooth, has no obvious pores, and is completely cured.

[0168] Figure 6 The cross-sectional morphology of the solid polymer electrolyte membrane material of Example 8. It can be seen that the thickness of the solid polymer electrolyte membrane is about 200 μm-300 μm.

[0169] Figure 7The AC impedance spectra of the solid polymer electrolyte membrane material at different temperatures of Example 4. As the temperature increases, the intrinsic impedance of the solid polymer electrolyte membrane material gradually decreases. This is because when the temperature is high, the mobility of the chain segments in the polymer matrix is ​​stronger. In this case, it is easier for the carriers to move in a directional manner with the chain segments, which is manifested in the electrochemical performance as a decrease in impedance and an increase in ionic conductivity.

[0170] Figure 8 This is the electrochemical stability window obtained by testing the solid polymer electrolyte membrane material of Example 4 at room temperature. Since polysiloxane has good chemical stability, the prepared solid polymer electrolyte membrane material has a wider electrochemical stability window. Fig. 9 This is a curved picture of the solid polymer electrolyte membrane material of Example 8. Fig. 9 It can be seen that the obtained material has good flexibility.

[0171] Fig.10 is the thermal weight loss curve of the solid polymer electrolyte membrane material of Example 8. Fig.10 It can be seen that the obtained material has good heat resistance.

[0172] The above is an exemplary description of the embodiments of the present invention. However, the protection scope of the present invention is not limited to the above embodiments. Any modification, equivalent substitution, improvement, etc. made by those skilled in the art within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A polysiloxane comprising at least one polymer having a structure as shown in Formula I; in, R1, R2 and R3 are the same or different and are independently selected from C 1-6 Alkyl, C 6-12 Aryl substituted C 1-6 Alkyl, C 6-12 Aryl, at least one C 1-6 Alkyl substituted C 6-12 Aryl; R4 is selected from CN, CHO, nitro, amino, COOH, halogen or C 1-6 alkyl, provided that the C 1-6 The alkyl group is substituted by one, two or more of the following groups: CN, CHO, nitro, amino, COOH or halogen; Each R5 is the same or different and is independently selected from C 1-6 Alkyl, C 6-12 Aryl substituted C 1-6 Alkyl, C 6-12 Aryl, at least one C 1-6 Alkyl substituted C 6-12 Aryl, -C 1-6 Alkyl-acrylate, -C 1-6 Alkyl-methacrylate or -OC 1-6 Alkyl-C 2-4 Epoxyalkyl; provided that at least one of the R5 at both ends of the polymer in Formula Ⅰ is selected from one of the following groups: -C 1-6 Alkyl-acrylate, -C 1-6 Alkyl-methacrylate or -OC 1-6 Alkyl-C 2-4 Epoxyalkyl.

2. The polysiloxane according to claim 1, characterized in that m+n is any integer greater than 0 and less than or equal to 1000, and m is not 0.

3. The polysiloxane according to claim 1, characterized in that R1, R2 and R3 are the same or different and are each independently selected from methyl, ethyl, ethylphenyl, 2,4-dimethylphenyl or benzyl; R4 is selected from nitro, amino, -CH2X, -CH(X)CH3, -CH2CH2X, -CY3, -CH(Y)CH(Y)2, -C(Y)2CH2Y, wherein X is selected from -CN, amino, -C(=O)H, -COOH or halogen, and Y is selected from halogen; Each R5 is the same or different and is independently selected from methyl, ethyl, -(CH2)3OC(=O)C(CH3)=CH2, -(CH2)3OC(=O)CH=CH2 or -OCH2(CHCH2O), provided that at least one of the R5 groups at both ends of the polymer in Formula I is -(CH2)3OC(=O)C(CH3)=CH2, -(CH2)3OC(=O)CH=CH2 or -OCH2(CHCH2O).

4. The polysiloxane according to claim 1, characterized in that m is any integer between 1 and 1000, and n is any integer between 0 and 999.

5. The polysiloxane according to any one of claims 1 to 4, characterized in that The polymer having the structure shown in formula I has a structure shown in any one of the following formulas Ⅰ-A, Ⅰ-B, Ⅰ-C, Ⅰ-D, Ⅰ-E, and Ⅰ-F: In formulas Ⅰ-A, Ⅰ-B, Ⅰ-C, Ⅰ-D, Ⅰ-E and IF, m and n have the definitions as described in any one of claims 1-4.

6. The polysiloxane according to any one of claims 1 to 5, characterized in that The dielectric constant of the polysiloxane is 2-20 (10 5 Hz).

7. The method for preparing the photocurable polysiloxane according to any one of claims 1 to 6, characterized in that: The method comprises the following steps: using a cyclosiloxane monomer having a polar side chain substitution and having a structure shown in formula II and a compound having a structure shown in formula III as an end-capping agent to carry out a ring-opening polymerization reaction under the action of a catalyst to obtain a polysiloxane shown in formula I; In formula II, a+b is any integer greater than 2 and less than or equal to 6, and a is not 0; R1, R2, R3, and R4 have the definitions described in any one of claims 1 to 4; In formula III, R5 has the definition as defined in any one of claims 1-4.

8. Use of the photocurable polysiloxane according to any one of claims 1 to 4 in the preparation of solid polymer electrolyte membrane materials for lithium ion batteries.

9. A solid polymer electrolyte material for lithium ion batteries, characterized in that: include: The photocurable polysiloxane, lithium salt and photoinitiator according to any one of claims 1 to 4.

10. The solid polymer electrolyte material for lithium ion batteries according to claim 9, characterized in that: The lithium salt is LiNO3, LiClO4, LiBF4, LiAsF6, LiPF6, LiBOB, LiDFOB, LiFSI, LiTFSI, LiSbF6, LiN(C4F9SO2)2, LiCF3CO2, LiAlCl4, Li2B 12 F 12 , LiCF3SO3 or more.

Citation Information

Patent Citations

  • Composite all solid-state polymer electrolyte lithium ion battery and preparation method of composite all solid-state polymer electrolyte lithium ion battery

    CN102709597A

  • Solid-state lithium battery silicon dioxide aerogel framework electrolyte and preparation method thereof

    CN111916818A

  • Polymer electrolyte

    CN116686115A

  • Polysiloxane Comb-branched with Alkyl Cyanide groupsand / or their Preparation for Solid PolymerElectrolytes.