Modified nanocellulose reinforced biodegradable composite film and preparation method thereof
By adding hydrophobically modified nanocellulose to PLA and PPC, the problem of poor material compatibility is solved, the mechanical and hydrophobic properties of the composite membrane are significantly improved, and the high-performance preparation of biodegradable composite membrane is achieved, suitable for grinding membranes and food packaging.
Patent Information
- Application Number
- CN202410931374.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-07-12
AI Technical Summary
Due to the large polarity difference and poor compatibility of existing PLA and PPC blend materials, the mechanical properties are poor, and the difficulty of uniform dispersion of nanocellulose nanocrystals in the polyester matrix is limited, which limits its in biodegradable composite membranes. Application.
After treating nanoscale microcrystalline cellulose in aqueous sodium periodate solution, dodecanediamine is added to react to form hydrophobically modified nanocellulose, and blended with PLA and PPC, using cast coating film Method to prepare biodegradable composite membrane to improve its compatibility and crystallization properties.
It significantly improves the mechanical properties and hydrophobic properties of the composite film, with strength reaching 34.9MPa and elongation at break reaching 46.9%. It is suitable for plastic film and food packaging, replacing traditional petroleum-based plastics.
Smart Images

Figure CN118994666A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of biodegradable composite films, and particularly relates to a modified nanocellulose reinforced biodegradable composite film and a preparation method thereof. Background Art
[0002] Petroleum-based synthetic plastics are widely used in various plastic film products due to their suitable functional properties. However, the pollution caused by their non-degradability directly or indirectly affects the global carbon cycle, biodiversity and ecosystem stability. One of the most effective solutions is to develop biodegradable and eco-friendly materials to reduce environmental impact and replace petroleum-based plastics. Therefore, the fields of ground film, food packaging, etc. urgently need a biodegradable composite film material with simple preparation, low cost and excellent performance.
[0003] Polylactic acid (PLA) is a linear polyester polymerized from lactic acid. It is a completely biodegradable material with great application prospects in the fields of biomedicine, tissue engineering, packaging materials, etc. However, PLA has a slow crystallization rate, low crystallinity, poor impact resistance and elongation at break, which limits its further promotion and application, and often requires modification during the molding process. Polypropylene carbonate (PPC) is a biodegradable polymer material. PPC has the advantages of high elongation at break and good flexibility. In addition, propylene oxide and "greenhouse gas" CO2 are used as raw materials during synthesis, which alleviates the problems of greenhouse effect and white pollution. Through the method of blending PLA and PPC, PPC is used to improve the crystallization ability and toughness of PLA. However, due to the large difference in polarity between PLA and PPC, the two are partially compatible. Poor compatibility will significantly reduce the overall mechanical properties of the material. Therefore, it is very necessary to improve the crystallization ability of PLA while ensuring good compatibility in modified PLA materials.
[0004] Cellulose nanocrystals (CNC) are one of the most promising nanomaterials. They have excellent rigidity, adjustable aspect ratio, abundant hydroxyl groups, and are renewable. They are widely used as reinforcing fillers and bulking materials for PLA and PPC. However, the hydroxyl groups on the surface of cellulose nanocrystals will cause the cellulose nanocrystals to self-aggregate and easily agglomerate in the polyester matrix. In addition, their high hydrophilicity makes them incompatible with the hydrophobic bio-polyester matrix, further limiting the uniform dispersion of cellulose nanocrystals in the matrix. Summary of the invention
[0005] Based on the above-mentioned shortcomings and deficiencies in the prior art, one of the objects of the present invention is to at least solve one or more of the above-mentioned problems in the prior art. In other words, one of the objects of the present invention is to provide a modified nanocellulose reinforced biodegradable composite film and a preparation method thereof that meets one or more of the aforementioned needs.
[0006] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:
[0007] A method for preparing a modified nanocellulose reinforced biodegradable composite film comprises the following steps:
[0008] (1) dispersing nano-sized microcrystalline cellulose in a sodium periodate aqueous solution, reacting at 60-80° C. for 50-60 min, cooling the reaction product to room temperature, washing, and drying to obtain aldehyde-containing nanocellulose;
[0009] (2) dispersing the aldehyde-containing nanocellulose in deionized water, adjusting the pH value to 4-5, adding dodecanediamine, reacting the mixture at 20-40° C. for 20-30 hours, cooling the reaction product to room temperature, washing, and drying to obtain modified nanocellulose;
[0010] (3) dissolving polylactic acid and polypropylene carbonate in chloroform to obtain a mixed solution, dispersing modified nanocellulose in chloroform to obtain a dispersion solution, stirring the mixed solution and the dispersion solution to obtain a film-forming solution, casting the film-forming solution, and drying to obtain a biodegradable composite film.
[0011] The invention uses hydrophobically modified nanocellulose as a reinforcing agent and a compatibilizer to improve the compatibility of PLA and PPC and the crystallization performance of PLA. Dodecane diamine DDA is used as a hydrophobically modified substance. DDA is a long-chain alkylamine with a relatively long hydrophobic alkyl chain. When DDA reacts with nanocellulose, the number of formed hydrophobic alkyl chains is relatively large, while the number of generated hydrogen bonds is relatively small. Therefore, there are more hydrophobic groups in the product, and the molecules are more inclined to repel water, so that the modified cellulose nanocrystals show hydrophobicity. Therefore, the invention uses DDA as a hydrophobically modified reinforcing agent and a compatibilizer to prepare a reinforced and toughened biodegradable PLA / PPC composite film, so as to be applied to the fields of degradable food packaging, ground film and other materials.
[0012] As a preferred embodiment, in the step (2), the mass ratio of the aldehyde-containing nanocellulose to dodecanediamine is 1:(1-3).
[0013] As a preferred embodiment, in the step (3), the mass ratio of polylactic acid to polypropylene carbonate is (60-70):(30-40).
[0014] As a preferred embodiment, in the step (3), the mass ratio of polylactic acid, polypropylene carbonate and chloroform is 1:(2-4), and the mixture is heated to 50-60°C and stirred to dissolve to obtain a mixed solution.
[0015] As a preferred embodiment, in step (3), the mass ratio of modified nanocellulose to chloroform in the dispersion is 1:(80-200).
[0016] As a preferred embodiment, the mass ratio of the nano-scale microcrystalline cellulose to the sodium periodate aqueous solution is 1:(90-110).
[0017] As a preferred embodiment, the concentration of the sodium periodate aqueous solution is 0.5-1M.
[0018] The present invention also provides a modified nanocellulose reinforced biodegradable composite film prepared by the preparation method described in any of the above schemes.
[0019] As a preferred solution, the mass fraction of the modified nanocellulose in the biodegradable composite film is 1 to 5 wt %.
[0020] As a preferred embodiment, the biodegradable composite film is used as ground film or food packaging.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] (1) The modified nanocellulose used in the present invention has the advantages of wide raw material sources, simple preparation process, low energy consumption, and biodegradability in terms of preparation, and has the advantages of high crystallinity, high specific surface area, and light weight in terms of structure, and can be widely used as an excellent reinforcing agent;
[0023] (2) The biodegradable composite film of the present invention uses a simple cast film preparation method, mature technology, and is easy to mass produce; the composite film has the advantages of good biocompatibility and high degradation rate, especially a strength of 34.9 MPa and an elongation at break of 46.9%, and has significantly improved crystallization ability and hydrophobic properties. It can replace traditional petroleum-based plastic films and some similar degradable plastic films on the market to a certain extent, and can be used in the fields of ground films, food packaging, etc., with a large market demand and considerable social and economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a field emission scanning electron microscope photograph of the modified nanocellulose of Example 2 of the present invention;
[0025] Figure 2 This is the infrared spectrum of the modified nanocellulose of Example 2 of the present invention;
[0026] Figure 3 This is a comparison diagram of contact angle tests of modified nanocellulose and nanocellulose in Example 2 of the present invention and Comparative Example 1;
[0027] Figure 4 The figures are the mechanical tensile test diagrams of the composite films of various embodiments and comparative examples of the present invention;
[0028] Figure 5The contact angle test diagram of the composite film of each embodiment of the present invention is shown in FIG. DETAILED DESCRIPTION
[0029] The technical solution of the present invention is further explained below through specific embodiments.
[0030] Embodiment 1:
[0031] The composite film P of this embodiment 70 / P 30 The preparation method comprises the following steps:
[0032] (1) dispersing 1 part by weight of nano-scale microcrystalline cellulose MCC in 10.69 parts by weight of sodium periodate aqueous solution (concentration 0.5 M), reacting at 60° C. for 60 min, cooling to room temperature after the reaction, washing, and drying to obtain aldehyde-containing nanocellulose CNC;
[0033] (2) The mass ratio of polylactic acid (PLA) and poly(propylene carbonate) (PPC) was 70:30, and the mass ratio of polylactic acid, poly(propylene carbonate) and chloroform solution was 1:6. The mixture was stirred and dissolved under the condition of heating to 60°C. The dissolved PLA / PPC chloroform mixture was stirred at room temperature for 24 hours until it was fully dispersed. The PLA / PPC chloroform mixture was cast and dried in an oven at 35°C for 48 hours to obtain a reinforced, toughened and degradable composite film, referred to as P 70 / P 30 .
[0034] Embodiment 2:
[0035] The preparation method of the composite film 1% CNC-DDA of this embodiment comprises the following steps:
[0036] (1) dispersing 1 part by weight of nano-scale microcrystalline cellulose MCC in 10.69 parts by weight of sodium periodate aqueous solution (concentration 0.5 M), reacting at 60° C. for 60 min, cooling to room temperature after the reaction, washing, and drying to obtain aldehyde-containing nanocellulose CNC;
[0037] (2) dispersing 1 part by mass of nanocellulose in deionized water, adjusting the pH value to 4.5, adding 2 parts by mass of dodecanediamine, reacting the mixture at 30° C. for 24 h, cooling the reaction product to room temperature, washing to neutrality, and drying to obtain modified nanocellulose CNC-DDA;
[0038] (3) The mass ratio of polylactic acid to polypropylene carbonate is 70:30, and the mass ratio of polylactic acid to polypropylene carbonate to chloroform solution is 1:4, and the mixture is stirred and dissolved under the condition of heating to 60° C. to obtain a polylactic acid / polypropylene carbonate chloroform mixed solution;
[0039] The mass ratio of modified nanocellulose to chloroform is 1:200, and the obtained dispersion is ultrasonicated until it is uniformly dispersed. The polylactic acid / polypropylene carbonate chloroform mixed solution and the modified nanocellulose chloroform dispersion are mixed and stirred at room temperature for 24 hours until they are fully dispersed. The PLA / PPC / CNC-DDA chloroform solution is cast and coated, and dried in an oven at 35°C for 48 hours to obtain a reinforced, toughened and degradable composite film, referred to as 1% CNC-DDA. Among them, the mass of modified nanocellulose CNC-DDA accounts for 1% of the total mass of the composite film.
[0040] Embodiment 3:
[0041] The preparation method of the composite film 3% CNC-DDA of this embodiment comprises the following steps:
[0042] (1) dispersing 1 part by weight of nano-scale microcrystalline cellulose MCC in 10.69 parts by weight of sodium periodate aqueous solution (concentration 0.5 M), reacting at 60° C. for 60 min, cooling to room temperature after the reaction, washing, and drying to obtain aldehyde-containing nanocellulose CNC;
[0043] (2) dispersing 1 part by mass of nanocellulose in deionized water, adjusting the pH value to 4.5, adding 2 parts by mass of dodecanediamine, reacting the mixture at 30° C. for 24 h, cooling the reaction product to room temperature, washing to neutrality, and drying to obtain modified nanocellulose CNC-DDA;
[0044] (3) the mass ratio of polylactic acid to polypropylene carbonate is 70:30, the mass ratio of polylactic acid to polypropylene carbonate to chloroform solution is 1:3.09, and the mixture is stirred and dissolved under the condition of heating to 60° C. to obtain a polylactic acid / polypropylene carbonate chloroform mixed solution;
[0045] The mass ratio of modified nanocellulose to chloroform of the dispersion is 1:100, and the obtained dispersion is ultrasonicated until it is uniformly dispersed, the polylactic acid / polypropylene carbonate chloroform mixed solution and the modified nanocellulose chloroform dispersion are mixed and stirred at room temperature for 24 hours until they are fully dispersed, the PLA / PPC / CNC-DDA chloroform solution is cast and coated, and dried in an oven at 35°C for 48 hours to obtain a composite film, referred to as 3% CNC-DDA. Among them, the mass of modified nanocellulose (CNC-DDA) is required to account for 3% of the total mass of the composite film.
[0046] Embodiment 4:
[0047] The preparation method of the composite film 5% CNC-DDA of this embodiment comprises the following steps:
[0048] (1) dispersing 1 part by weight of nano-scale microcrystalline cellulose MCC in 10.69 parts by weight of sodium periodate aqueous solution (concentration 0.5 M), reacting at 60° C. for 60 min, cooling to room temperature after the reaction, washing, and drying to obtain aldehyde-containing nanocellulose CNC;
[0049] (2) dispersing 1 part by mass of nanocellulose in deionized water, adjusting the pH value to 4.5, adding 2 parts by mass of dodecanediamine, reacting the mixture at 30° C. for 24 h, cooling the reaction product to room temperature, washing to neutrality, and drying to obtain modified nanocellulose CNC-DDA;
[0050] (3) The mass ratio of polylactic acid to polypropylene carbonate is 70:30, and the mass ratio of polylactic acid to polypropylene carbonate to chloroform solution is 1:2, and the mixture is stirred and dissolved under the condition of heating to 60° C. to obtain a polylactic acid / polypropylene carbonate chloroform mixed solution;
[0051] The mass ratio of modified nanocellulose to chloroform of the dispersion is 1:80, and the obtained dispersion is ultrasonicated until it is uniformly dispersed, the polylactic acid / polypropylene carbonate chloroform mixed solution and the modified nanocellulose chloroform dispersion are mixed and stirred at room temperature for 24 hours until they are fully dispersed, the PLA / PPC / CNC-DDA chloroform solution is cast and coated, and dried in an oven at 35°C for 48 hours to obtain a composite film, referred to as 5% CNC-DDA. Among them, the mass of modified nanocellulose (CNC-DDA) is required to account for 5% of the total mass of the composite film.
[0052] Comparative Example 1:
[0053] The preparation method of the composite film 3% CNC-PEI of this embodiment comprises the following steps:
[0054] (1) dispersing 1 part by weight of nano-scale microcrystalline cellulose MCC in 10.69 parts by weight of sodium periodate aqueous solution (concentration 0.5 M), reacting at 60° C. for 60 min, cooling to room temperature after the reaction, washing, and drying to obtain aldehyde-containing nanocellulose CNC;
[0055] (2) dispersing 1 part by weight of aldehyde-containing nanocellulose in deionized water, adjusting the pH value to 4.5, adding 2 parts by weight of polyethyleneimine, reacting at 50° C. for 24 h, and after the reaction is completed, cooling to room temperature, centrifuging, washing, and drying to obtain modified nanocellulose CNC-PEI;
[0056] (3) the mass ratio of polylactic acid to polypropylene carbonate is 70:30, the mass ratio of polylactic acid to polypropylene carbonate to chloroform solution is 1:3.09, and the mixture is stirred and dissolved under the condition of heating to 60° C. to obtain a polylactic acid / polypropylene carbonate chloroform mixed solution;
[0057] The mass ratio of modified nanocellulose to chloroform of the dispersion is 1:100, and the obtained dispersion is ultrasonicated until it is uniformly dispersed, the polylactic acid / polypropylene carbonate chloroform mixed solution and the modified nanocellulose chloroform dispersion are mixed and stirred at room temperature for 24 hours until they are fully dispersed, the PLA / PPC / CNC-PEI chloroform solution is cast and coated, and dried in an oven at 35°C for 48 hours to obtain a composite film, referred to as 3% CNC-PEI. Among them, the mass of modified nanocellulose CNC-PEI accounts for 3% of the total mass of the composite film.
[0058] like Figure 1 As shown, the modified nanocellulose grafted with dodecanediamine in Example 2 still presents a spherical shape. The modified nanocellulose obtained in other examples is the same as that in Example 2.
[0059] like Figure 2 The infrared spectrum of nanocellulose CNC is shown at 1732 cm -1 There is an obvious absorption peak of aldehyde group C=O, while the absorption peak of aldehyde group in the infrared spectrum of modified nanocellulose CNC-DDA almost disappears and is concentrated at 1644cm -1 A new absorption peak appeared, which came from CN stretching vibration, indicating that the amino group of dodecane diamine reacted with the aldehyde group on nanocellulose to form a Schiff base reaction; it can also be observed that after adding dodecane diamine DDA, the saturated CH bond of nanocellulose CNC became two saturated CH bonds, because the aldehyde group and the amino group formed an addition reaction, thereby converting the original saturated CH bond into two new chemical bonds. The above infrared results show that dodecane diamine was successfully grafted onto nanocellulose.
[0060] Figure 3 The contact angle test results show that the contact angle of CNC-DDA is significantly improved. The reason is that DDA is a long-chain alkylamine, which usually has a long hydrophobic alkyl chain. When DDA reacts with the aldehyde group of nanocellulose, the number of hydrophobic alkyl chains in the formed product is relatively large, while the number of hydrogen bonds produced is relatively small, which makes the product more hydrophobic overall. Due to the large number of hydrophobic groups in the product, the molecule tends to repel water, making it hydrophobic; while CNC-PEI exhibits hydrophilicity. The reason is that when the imine group in polyethylene imine reacts with the aldehyde group, the formed product has more hydroxyl and amine (amide) functional groups. These functional groups increase the hydrogen bonding between the molecular surface and water molecules, thereby enhancing the hydrophilicity of the molecule. In addition, the amine groups in the formed product can also form hydrogen bonds with water molecules, further enhancing the interaction with water molecules, making the product exhibit better hydrophilicity.
[0061] Figure 4The tensile test results show that the mechanical properties and elongation at break of the composite membrane with modified nanocellulose are significantly improved, and the strength of 3% CNC-DDA reaches 34.9MPa, which is higher than that of P 70 / P 30 The composite film increased by 78.9%, and the elongation at break reached 46.9%, with a relative increase of 31.3%, proving that the modified nanocellulose has an additional help in improving the compatibility of the system and the mechanical properties, and can be used as ground film or food packaging, etc.; the strength and elongation at break of 5% CNC-DDA are less than those of P 70 / P 30 The reason for the poor mechanical properties of the composite membrane is that the concentration of modified nanocellulose is too high, which is easy to agglomerate and reduces the mechanical properties. The reason for the poor mechanical properties of 3% CNC-PEI is that the highly hydrophilic modified nanocellulose is incompatible with the hydrophobic biopolyester matrix, which further limits the uniform dispersion of cellulose nanocrystals in the matrix.
[0062] Figure 5 The contact angle test results show that the hydrophobic properties of the composite membrane have been greatly improved after adding modified nanocellulose, which benefits from the successful preparation of hydrophobic modified nanocellulose.
[0063] In view of the numerous embodiments of the scheme of the present invention, the raw materials and dosage involved can be selected according to actual needs within the limited range, and the experimental data of each embodiment is huge and numerous, which is not suitable for listing and explaining one by one here, but the content required to be verified and the final conclusion obtained in each embodiment are similar. Therefore, the verification content of each embodiment will not be explained one by one here.
[0064] The above description is only a detailed description of the preferred embodiments and principles of the present invention. For ordinary technicians in this field, according to the ideas provided by the present invention, there will be changes in the specific implementation methods, and these changes should also be regarded as the protection scope of the present invention.
Claims
1. A method for preparing a modified nanocellulose reinforced biodegradable composite film, characterized in that: The following steps are involved: (1) dispersing nano-sized microcrystalline cellulose in a sodium periodate aqueous solution, reacting at 60-80° C. for 50-60 min, cooling the reaction product to room temperature, washing, and drying to obtain aldehyde-containing nanocellulose; (2) dispersing the aldehyde-containing nanocellulose in deionized water, adjusting the pH value to 4-5, adding dodecanediamine, reacting the mixture at 20-40° C. for 20-30 hours, cooling the reaction product to room temperature, washing, and drying to obtain modified nanocellulose; (3) dissolving polylactic acid and polypropylene carbonate in chloroform to obtain a mixed solution, dispersing modified nanocellulose in chloroform to obtain a dispersion solution, stirring the mixed solution and the dispersion solution to obtain a film-forming solution, casting the film-forming solution, and drying to obtain a biodegradable composite film.
2. The preparation method according to claim 1, characterized in that: In the step (2), the mass ratio of the aldehyde-containing nanocellulose to dodecanediamine is 1:(1-3).
3. The preparation method according to claim 1, characterized in that: In the step (3), the mass ratio of polylactic acid to polypropylene carbonate is (60-70):(30-40).
4. The preparation method according to claim 1, characterized in that: In the step (3), the mass ratio of polylactic acid, polypropylene carbonate and chloroform is 1:(2-4), heated to 50-60° C., stirred and dissolved to obtain a mixed solution.
5. The preparation method according to claim 1, characterized in that: In the step (3), the mass ratio of the modified nanocellulose to chloroform in the dispersion is 1:(80-200).
6. The preparation method according to claim 1, characterized in that: The mass ratio of the nano-scale microcrystalline cellulose to the sodium periodate aqueous solution is 1:(90-110).
7. The preparation method according to claim 6, characterized in that: The concentration of the sodium periodate aqueous solution is 0.5-1M.
8. The modified nanocellulose reinforced biodegradable composite film prepared by the preparation method according to any one of claims 1 to 7.
9. The biodegradable composite film according to claim 8, characterized in that: The mass fraction of the modified nanocellulose in the biodegradable composite film is 1 to 5 wt %.
10. The biodegradable composite film according to claim 8 or 9, characterized in that: Used as mulch or food packaging.
Citation Information
Patent Citations
Modified nanocellulose as well as preparation method and application thereof
CN108219009A
High-transparency and high-strength nanocellulose flexible film as well as preparation method and application thereof
CN113402745A
High-barrier biodegradable material, and preparation method and application thereof
CN113861643A
Modified cellulose nanocrystal as well as preparation method and application thereof
CN115716882A
Biodegradable polylactic acid toughening and reinforcing material for injection molding and injection molding product based on biodegradable polylactic acid toughening and reinforcing material
CN115785631A