Vinyl hyperbranched siloxane modified polyimide porous composite material and preparation method thereof

By using vinyl superbranched silicone to modify polyimide porous composite materials in the preparation of polyimide porous materials, the problem of complicated preparation methods and poor performance in the prior art is solved, and uniform pore size is achieved , low-cost industrial production of polyimide porous materials with excellent mechanical properties, suitable for microelectronics and aerospace fields.

CN118994713APending Publication Date: 2024-11-22NANJING UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411091998.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the prior art, the preparation method of polyimide porous materials is complicated, easy to contaminate, poor performance, difficult to achieve industrial production, uncontrollable pore size, high cost, and the solvent used in the prior art consumes time, affecting large-scale production. .

Method used

By reacting diamine, acid anhydride and unsaturated monoanhydride in a polar solvent, an unsaturated anhydride-capped polyamic acid solution is formed, and after adding vinyl hyperbranched silicone, casting and imidizing, the pore size is prepared. A uniform and excellent mechanical properties of vinyl hyperbranched silicone modified polyimide porous composite material.

Benefits of technology

It realizes the preparation of simple and low-cost polyimide porous materials, with uniform pore size, excellent temperature resistance and mechanical properties, and is suitable for industrial production, and has expanded applications in microelectronics, aerospace and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994713A_ABST
    Figure CN118994713A_ABST
Patent Text Reader

Abstract

The invention discloses a vinyl hyperbranched siloxane modified polyimide porous composite material and a preparation method thereof.The preparation method comprises the following steps that firstly, diamine, dianhydride and unsaturated monoanhydride react in a polar solvent, and an unsaturated anhydride terminated polyamide acid solution is obtained; step 2, adding vinyl hyperbranched siloxane into the solution obtained in the step 1, and reacting to obtain a vinyl hyperbranched siloxane modified unsaturated anhydride terminated PAA solution; and step 3, casting the solution obtained in the step 2 on a substrate, drying the solvent, and heating for imidization. In the first step, the molar ratio of diamine to dianhydride to unsaturated monoanhydride is 1: (0.5-0.9): (0.2-1). The obtained vinyl hyperbranched siloxane / polyimide microporous material is uniform in pore diameter and excellent in temperature resistance and mechanical performance, and the mechanical performance of the polyimide material can be further improved through introduction of vinyl hyperbranched siloxane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to a polymer composite material and a preparation method thereof, in particular to a vinyl hyperbranched siloxane modified polyimide porous composite material and a preparation method thereof. Background Art

[0002] Polyimide porous material is a kind of porous material with polyimide as the main body and a certain open or closed pore structure inside. It has adjustable density (5-400kg / m 3 ), excellent mechanical properties, excellent thermal properties, chemical resistance, etc., and has been widely used in filtration separation, microelectronics, aerospace, energy storage and conversion and other fields.

[0003] Common methods for preparing polyimide porous materials mainly include phase separation method, template method, chemical etching and chemical vapor deposition technology. Chinese patent CN115746380A discloses a method for preparing a polyimide porous composite material, which adopts an in-situ polymerization method to mix nano-scale silica microspheres (SiO2), nickel powder or one of ionic liquids with a solvent and diamine, dianhydride for a period of time to obtain a polyamic acid (PAA) solution with nano-SiO2, nickel powder or ionic liquid, and then prepares a porous PI composite material through casting, drying, imidization, etching and other processes. Although this method can obtain a polyimide porous material with uniform pore size, it needs to use HF or HCl for long-term etching, and the process is cumbersome and prone to environmental pollution. Chinese patent CN 115322431 A discloses a low dielectric cross-linked porous polyimide material and a preparation method thereof, which mainly comprises the following steps: copolymerizing a diamine monomer containing a cross-linkable group with other diamine monomers and a dianhydride monomer to obtain a cross-linked polyimide; dissolving the cross-linked polyimide and a porogen in a solvent to obtain a uniform polymer solution, casting the solution on a clean substrate, subjecting the solution to programmed heating and thermal cross-linking treatment to obtain a cross-linked polyimide material, and then washing away the porogen in a solvent to obtain a low dielectric cross-linked porous polyimide material. The dielectric constant of the porous polyimide material obtained by the method is less than 2.5 at 1 MHz, which broadens the application of polyimide in the fields of microelectronics and communications. However, a large amount of solvent needs to be used in the pore-making process. At the same time, since the penetration rate of the solvent in the cross-linked polyimide material is relatively low, the pore-making time is long and the pore size is uncontrollable. CN 114426698 A discloses an ultra-low dielectric porous polyimide material and a preparation method thereof. The material is prepared by in-situ polymerization and blending using aromatic dianhydride and diamine as polymerization monomers and ionic liquid 1-butyl-3-methylimidazolium tetrafluoroborate as a porogen. The material is then immersed in an organic solvent to remove the ionic liquid to obtain a porous polyimide material with an ultra-low dielectric constant, good thermal stability and excellent hydrophobic properties. Although the ionic liquid is added to form pores so that the uniformity of the pores is guaranteed, the ionic liquid has a high cost and requires a long time to be immersed in an organic solvent, which is not conducive to large-scale production. CN 103422253 B discloses a highly polyimide porous membrane containing benzimidazole and benzene side groups and a preparation method thereof. The method mainly comprises the following steps: electrospinning a polyamic acid containing benzimidazole and benzene side groups to obtain a polyamic acid porous membrane, and then subjecting the polyamic acid to thermal imidization to obtain a polyimide porous membrane. The novel polyimide porous material can be widely used in battery separators, capacitor separators, air purification and other fields. However, the diamine monomer containing benzimidazole and benzene side groups is expensive, and the electrospinning equipment is expensive, so industrialization has not been achieved.

[0004] At present, there are few commercial polyimide porous materials in China and their performance is poor. Most of the polyimide porous materials prepared in the existing technology use templates or etching methods, which are time-consuming and pollute the environment, and the comprehensive performance cannot meet the use requirements. Therefore, how to provide a simple, convenient, green and environmentally friendly preparation method of polyimide porous materials and further improve the various properties of polyimide porous materials is of great significance. Summary of the invention

[0005] Purpose of the invention: In order to overcome the deficiencies in the prior art, the purpose of the present invention is to provide a method for preparing a vinyl hyperbranched siloxane-modified polyimide porous composite material which is simple, convenient, low-cost and easy to industrialize. Another purpose of the present invention is to provide a vinyl hyperbranched siloxane-modified polyimide porous composite material with uniform pore size, excellent temperature resistance and excellent mechanical properties.

[0006] Technical solution: The method for preparing a vinyl hyperbranched siloxane modified polyimide porous composite material of the present invention comprises the following steps:

[0007] Step 1, reacting a diamine, a dianhydride and an unsaturated monoanhydride in a polar solvent to obtain an unsaturated anhydride-terminated polyamic acid solution;

[0008] Step 2, adding vinyl hyperbranched siloxane to the solution obtained in step 1, and reacting to obtain a vinyl hyperbranched siloxane-modified unsaturated anhydride-terminated PAA solution;

[0009] Step three, casting the solution obtained in step two on a substrate, drying the solvent and then heating to perform imidization, so as to obtain a vinyl hyperbranched siloxane modified polyimide porous composite material.

[0010] Furthermore, in step 1, the molar ratio of diamine, dianhydride and unsaturated monoanhydride is 1:0.5-0.9:0.2-1.

[0011] Further, the diamine is one or more of 4,4'-diaminodiphenyl ether, 2,6-diaminopyridine, 4,4'-diaminodiphenyl sulfone, m-phenylenediamine, p-phenylenediamine, 4,4'-bis(3-aminophenoxy)biphenyl, 2,5-bis(4-aminophenyl)pyridine, bisphenol A diether diamine, and 1,3-bis(3-aminopropyl)tetramethyldisiloxane. The specific general formula is as follows:

[0012]

[0013] Furthermore, in step 1, the dianhydride is one or more of pyromellitic anhydride, 3,3',4,4'-diphenylsulfone tetracarboxylic anhydride, 2,3,3',4'-diphenyl ether tetracarboxylic anhydride, 3,3',4,4'-diphenyl ether tetracarboxylic anhydride, 3,3',4,4'-diphenyl ether tetracarboxylic anhydride, 3,3',4,4'-benzophenone tetracarboxylic anhydride, 3,3',4,4'-biphenyltetracarboxylic anhydride, and hexafluoro dianhydride. The specific general formula is as follows:

[0014]

[0015] Furthermore, in step one, the unsaturated monoanhydride is one or more of maleic anhydride, dimethylmaleic anhydride, methylmaleic anhydride, 2,3-dichloromaleic anhydride, nadic anhydride, methylnadic anhydride, dimethylnadic anhydride, and 2-hexyl-3-methylmaleic anhydride.

[0016] Furthermore, in step 1, the polar solvent is one or more of N-methylpyrrolidone, N-ethylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, and dimethyl sulfoxide, and the mass percentage of the polar solvent is 60 to 90 wt%.

[0017] Furthermore, in step 1, the reaction temperature is -30 to 80°C, and the reaction time is 1 to 24 hours. The reaction temperature is preferably -10 to 50°C.

[0018] Further, in step 2, the mass ratio of the vinyl hyperbranched siloxane to the solution obtained in step 1 is 0.01 to 0.6:1, the double bond content of the vinyl hyperbranched siloxane is 1 to 15wt%, the reaction temperature is -20 to 70°C, and the reaction time is 1 to 12h. Preferably, the mass ratio of the vinyl hyperbranched siloxane to the solution obtained in step 1 is 0.05 to 0.5:1, the reaction temperature is 0 to 25°C, and the reaction time is 2 to 6h.

[0019] The general formula of vinyl hyperbranched siloxane is:

[0020]

[0021] R' is one or more of methyl, ethyl, trifluoromethyl and phenyl.

[0022] Furthermore, in step 3, the temperature of drying the solvent is 40-100°C for 1-12 hours, and the temperature of imidization is 180-400°C for 1-8 hours. Preferably, the temperature of drying the solvent is 50-90°C for 4-10 hours, and the temperature of imidization is 250-350°C for 2-6 hours.

[0023] The vinyl hyperbranched siloxane modified polyimide porous composite material of the invention has a pore diameter of 1 to 7.1 micrometers and a porosity of 72.3 to 90%.

[0024] Preparation principle: It is mainly through the formation of microphase separation of vinyl hyperbranched siloxane in the unsaturated anhydride-terminated polyamic acid solution. At the same time, during the evaporation of the solvent, the vinyl hyperbranched siloxane can undergo further cross-linking, maintaining the porous structure of the film material, further increasing the cross-linking density of the hybrid film material, and improving the mechanical strength of the film material.

[0025] Beneficial effects: Compared with the prior art, the present invention has the following significant features:

[0026] 1. The obtained vinyl hyperbranched siloxane / polyimide microporous material has uniform pore size, excellent temperature resistance and mechanical properties, and the introduction of vinyl hyperbranched siloxane can further improve the mechanical properties of the polyimide material;

[0027] 2. This method has a simple synthesis process, low cost, and is easy to realize industrial production. It has industrial prospects and can further expand the application of polyimide materials in microelectronics, aerospace, and catalytic filtration. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a physical picture of the material obtained by the present invention;

[0029] Figure 2 is a scanning electron microscope image of the material obtained in the present invention;

[0030] Figure 3 is an infrared image of the material obtained in the present invention;

[0031] Figure 4 is a thermal stability diagram of the material obtained in the present invention;

[0032] Figure 5 is a dielectric constant spectrum of the material obtained by the present invention;

[0033] Figure 6 It is the XPS spectrum of the material obtained in the present invention. DETAILED DESCRIPTION

[0034] Unless otherwise specified, the materials, reagents, instruments, etc. used in the following examples can be obtained from commercial sources.

[0035] The experimental methods without specific conditions in the examples are usually carried out under conventional conditions or conditions recommended by the manufacturers.

[0036] Example 1

[0037] A method for preparing a vinyl hyperbranched siloxane modified polyimide porous composite material comprises the following steps:

[0038] (1) In a 250 ml three-necked flask equipped with a mechanical stirrer, 20.02 g (0.1 mol) of 4,4-diaminodiphenyl ether, 19.63 g (0.09 mol) of pyromellitic anhydride, 1.961 g (0.02 mol) of maleic anhydride and 62.42 g of N,N-dimethylformamide were added, and the mixture was reacted at -30°C for 24 h to obtain an unsaturated anhydride-terminated polyamic acid (PAA) solution.

[0039] (2) 0.397 g of vinyl hyperbranched siloxane was added to the unsaturated anhydride terminated PAA solution, and the mixture was reacted at -20°C for 12 hours to obtain a vinyl hyperbranched siloxane modified unsaturated anhydride terminated PAA solution. The double bond content of the vinyl hyperbranched siloxane was 1 wt %. The specific structural formula is as follows:

[0040]

[0041] (3) A vinyl hyperbranched siloxane-modified unsaturated anhydride-terminated PAA solution was cast on a substrate, dried at 40° C. for 12 h to dry the solvent, and then heated to 180° C. for 8 h to perform imidization to obtain a vinyl hyperbranched siloxane-modified polyimide porous composite material. The vinyl hyperbranched siloxane-modified polyimide porous material has an average pore size of about 2 μm and a porosity of about 83.2%.

[0042] Example 2

[0043] A method for preparing a vinyl hyperbranched siloxane modified polyimide porous composite material comprises the following steps:

[0044] (1) In a 1000 ml three-necked flask equipped with a mechanical stirrer, 10.81 g (0.1 mol) of p-phenylenediamine, 16.11 g (0.05 mol) of 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 9.806 g (0.1 mol) of 2-hexyl-3-methylmaleic anhydride and 330.53 g of dimethyl sulfoxide were added, and the mixture was reacted at 80° C. for 1 h to obtain an unsaturated anhydride-terminated polyamic acid (PAA) solution.

[0045] (2) Add 27.76 g of vinyl hyperbranched siloxane to the unsaturated anhydride terminated PAA solution, react at 70° C. for 1 h, and obtain a vinyl hyperbranched siloxane modified unsaturated anhydride terminated PAA solution. The double bond content of the vinyl hyperbranched siloxane is 15 wt %, and the specific structural formula is as follows:

[0046]

[0047] (3) Casting a PAA solution terminated with an unsaturated anhydride modified vinyl hyperbranched siloxane on a substrate, drying the solution at 100° C. for 2 h to dry the solvent, and then heating the solution to 400° C. for 1 h to perform imidization to obtain a vinyl hyperbranched siloxane modified polyimide porous composite material. The vinyl hyperbranched siloxane modified polyimide porous material has an average pore size of about 4.32 μm and a porosity of about 79.2%.

[0048] Example 3

[0049] A method for preparing a vinyl hyperbranched siloxane modified polyimide porous composite material comprises the following steps:

[0050] (1) In a 250 ml three-necked flask equipped with a mechanical stirrer, 24.83 g (0.1 mol) of 4,4'-diaminodiphenyl sulfone, 19.12 g (0.065 mol) of 3,3',4,4'-biphenyltetracarboxylic dianhydride, 14.77 g (0.09 mol) of methylnadicarboxylic anhydride and 58.72 g of N,N-dimethylacetamide were added, and reacted at 0°C for 12 h to obtain an unsaturated anhydride-terminated polyamic acid (PAA) solution.

[0051] (2) Add 2.639 g of vinyl hyperbranched siloxane to the unsaturated anhydride terminated PAA solution, react at 0° C. for 12 h, and obtain a vinyl hyperbranched siloxane modified unsaturated anhydride terminated PAA solution. The double bond content of the vinyl hyperbranched siloxane is 5 wt %, and the specific structural formula is as follows:

[0052]

[0053] (3) Casting a PAA solution capped with unsaturated anhydride modified by vinyl hyperbranched siloxane on a substrate, drying the solution at 50°C for 10 h to dry the solvent, and then heating the solution to 350°C for 2 h to perform imidization to obtain a vinyl hyperbranched siloxane modified polyimide porous composite material. The vinyl hyperbranched siloxane modified polyimide porous material has an average pore size of about 5 μm and a porosity of about 90%.

[0054] Example 4

[0055] A method for preparing a vinyl hyperbranched siloxane modified polyimide porous composite material comprises the following steps:

[0056] (1) In a 500 ml three-necked flask equipped with a mechanical stirrer, 52.05 g (0.1 mol) of bisphenol A diether diamine, 25.0 g (0.085 mol) of 3,3',4,4'-biphenyltetracarboxylic dianhydride, 4.925 g (0.03 mol) of nadic anhydride and 327.9 g of N-methylpyrrolidone were added, and the mixture was reacted at 0° C. for 12 h to obtain an unsaturated anhydride-terminated polyamic acid (PAA) solution.

[0057] (2) 49.35 g of vinyl hyperbranched siloxane was added to the unsaturated anhydride terminated PAA solution, and the mixture was reacted at 25° C. for 6 h to obtain a vinyl hyperbranched siloxane modified unsaturated anhydride terminated PAA solution, wherein the double bond content of the vinyl hyperbranched siloxane was 10 wt %. The specific structural formula is as follows:

[0058]

[0059] (3) Casting a PAA solution capped with unsaturated anhydride modified by vinyl hyperbranched siloxane on a substrate, drying at 90°C for 4 hours to dry out the solvent, and then heating to 250°C for 6 hours to perform imidization to obtain a vinyl hyperbranched siloxane modified polyimide porous composite material. The vinyl hyperbranched siloxane modified polyimide porous material has an average pore size of about 3.72 μm and a porosity of about 83.6%.

[0060] Example 5

[0061] A method for preparing a vinyl hyperbranched siloxane modified polyimide porous composite material comprises the following steps:

[0062] (1) In a 500 ml three-necked flask equipped with a mechanical stirrer, 26.03 g (0.05 mol) of bisphenol A diether diamine, 10.012 g (0.05 mol) of 4,4-diaminodiphenyl ether, 12.5 g (0.0425 mol) of 3,3',4,4'-biphenyltetracarboxylic dianhydride, 9.44 g (0.0425 mol) of hexafluorodianhydride, 4.925 g (0.03 mol) of nadic anhydride and 327.9 g of N-methylpyrrolidone were added, and the mixture was reacted at 0° C. for 12 h to obtain an unsaturated anhydride-terminated polyamic acid (PAA) solution.

[0063] (2) Add 49.35 g of vinyl hyperbranched siloxane to the unsaturated anhydride terminated PAA solution, react at 25° C. for 6 h, and obtain a vinyl hyperbranched siloxane modified unsaturated anhydride terminated PAA solution. The double bond content of the vinyl hyperbranched siloxane is 10 wt %, and the specific structural formula is as follows:

[0064]

[0065] (3) Casting a PAA solution capped with unsaturated anhydride modified by vinyl hyperbranched siloxane on a substrate, drying at 90°C for 4 h to dry the solvent, and then heating to 250°C for 6 h to perform imidization to obtain a vinyl hyperbranched siloxane modified polyimide porous composite material. The vinyl hyperbranched siloxane modified polyimide porous material has an average pore size of about 7.1 μm and a porosity of about 72.3%.

[0066] Comparative Example 1

[0067] The remaining steps of this comparative example are the same as those of Example 1, except that maleic anhydride is replaced by cyclopentanoic anhydride.

[0068] Comparative Example 2

[0069] The remaining steps of this comparative example are the same as those of Example 1, except that the vinyl hyperbranched siloxane is replaced by amino hyperbranched siloxane.

[0070] Test Method

[0071] The density of the materials obtained in the above Examples 1 to 5 and Comparative Examples 1 to 2 was tested according to GB / T 26321-2010; the water contact angle was measured according to GBT 30693-2014; the initial thermal decomposition temperature was tested according to GB / T 4498.2; and the tensile property was tested according to GB / T 13542.6-2006.

[0072] Table 1 Performance data of materials obtained in Examples 1 to 5 and Comparative Examples 1 to 2

[0073]

[0074] like Figure 1 The vinyl hyperbranched siloxane modified polyimide porous composite material obtained in Example 4 has excellent flexibility, and the material will not break after being bent.

[0075] like Figure 2 The vinyl hyperbranched siloxane modified polyimide porous composite material obtained in Example 4 exhibits a uniform pore structure, and the average pore size is about 1 μm.

[0076] like Figure 3 The vinyl hyperbranched siloxane modified polyimide porous composite material obtained in Example 4 has a decomposition temperature of 10% as high as 460°C, and a residual carbon of up to 60% at 1000°C, showing excellent thermal stability.

[0077] like Figure 4 The tensile strength of the vinyl hyperbranched siloxane modified polyimide porous composite material obtained in Example 4 can be as high as 80 MPa, showing excellent mechanical strength.

[0078] like Figure 5 The dielectric constant of the vinyl hyperbranched siloxane modified polyimide porous composite material obtained in Example 4 is only 1.77, which is expected to further expand the application of polyimide film materials in rigid circuit boards.

[0079] Among the above embodiments, embodiment 4 is the best embodiment.

Claims

1. A method for preparing a porous composite material of vinyl hyperbranched siloxane modified polyimide, characterized in that: The following steps are involved: Step 1, reacting a diamine, a dianhydride and an unsaturated monoanhydride in a polar solvent to obtain an unsaturated anhydride-terminated polyamic acid solution; Step 2, adding vinyl hyperbranched siloxane to the solution obtained in step 1, and reacting to obtain a vinyl hyperbranched siloxane-modified unsaturated anhydride-terminated PAA solution; Step three, casting the solution obtained in step two on a substrate, drying the solvent and then heating to perform imidization, so as to obtain a vinyl hyperbranched siloxane modified polyimide porous composite material.

2. The method for preparing a porous composite material of vinyl hyperbranched siloxane modified polyimide according to claim 1, characterized in that: In the step 1, the molar ratio of diamine, dianhydride and unsaturated monoanhydride is 1:0.5-0.9:0.2-1.

3. The method for preparing a porous composite material of vinyl hyperbranched siloxane modified polyimide according to claim 1, characterized in that: In the step 1, the diamine is one or more of 4,4'-diaminodiphenyl ether, 2,6-diaminopyridine, 4,4'-diaminodiphenyl sulfone, m-phenylenediamine, p-phenylenediamine, 4,4'-bis(3-aminophenoxy)biphenyl, 2,5-bis(4-aminophenyl)pyridine, bisphenol A diether diamine, and 1,3-bis(3-aminopropyl)tetramethyldisiloxane.

4. The method for preparing a porous composite material of vinyl hyperbranched siloxane modified polyimide according to claim 1, characterized in that: In the step 1, the dianhydride is one or more of pyromellitic anhydride, 3,3',4,4'-diphenyl sulfone tetracarboxylic dianhydride, 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride, 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride, 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride, 3,3',4,4'-dibenzophenone tetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, and hexafluoro dianhydride.

5. The method for preparing a porous composite material of vinyl hyperbranched siloxane modified polyimide according to claim 1, characterized in that: In the step 1, the unsaturated monoanhydride is one or more of maleic anhydride, dimethylmaleic anhydride, methylmaleic anhydride, 2,3-dichloromaleic anhydride, nadic anhydride, methylnadic anhydride, dimethylnadic anhydride, and 2-hexyl-3-methylmaleic anhydride.

6. The method for preparing a porous composite material of vinyl hyperbranched siloxane modified polyimide according to claim 1, characterized in that: In the step 1, the polar solvent is one or more of N-methylpyrrolidone, N-ethylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, and dimethyl sulfoxide, and the mass percentage of the polar solvent is 60 to 90 wt%.

7. The method for preparing a porous composite material of vinyl hyperbranched siloxane modified polyimide according to claim 1, characterized in that: In the step 1, the reaction temperature is -30 to 80° C., and the reaction time is 1 to 24 hours.

8. The method for preparing a porous composite material of vinyl hyperbranched siloxane modified polyimide according to claim 1, characterized in that: In the step 2, the mass ratio of the vinyl hyperbranched siloxane to the solution obtained in the step 1 is 0.01-0.6:1, the double bond content of the vinyl hyperbranched siloxane is 1-15wt%, the reaction temperature is -20-70°C, and the reaction time is 1-12h.

9. The method for preparing a porous composite material of vinyl hyperbranched siloxane modified polyimide according to claim 1, characterized in that: In the step 3, the temperature of drying the solvent is 40-100° C. for 1-12 hours, and the temperature of imidization is 180-400° C. for 1-8 hours.

10. A porous composite material of vinyl hyperbranched siloxane modified polyimide obtained by the method for preparing a porous composite material of vinyl hyperbranched siloxane modified polyimide according to any one of claims 1 to 9, characterized in that: The pore diameter is 1 to 7.1 μm, and the porosity is 72.3 to 90%.

Citation Information

Cited By

  • High-temperature-resistant high-energy-storage-density silicon-containing polyimide dielectric thin film material and preparation method thereof

    CN121378742A