Antibacterial fiber sponge material and preparation method thereof

By introducing raw materials such as graphene oxide fibers into sponge materials, antibacterial fiber sponges with multiple interpenetrating network structures are formed, which solves the problems of insufficient antibacterial stability and mechanical properties, achieves significant antibacterial effects and resistance to damp heat aging, and extends service life.

CN118240323BActive Publication Date: 2024-11-19YANGZHOU ZHONGTIAN SPONGE CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410452643.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-16
Publication Date
2024-11-19
Estimated Expiration
2044-04-16

AI Technical Summary

Technical Problem

Existing antibacterial sponge materials suffer from insufficient antibacterial stability, limited mechanical properties, poor feel, short service life, and poor resistance to damp heat aging.

Method used

Antibacterial fiber sponge materials with various interpenetrating network structures are formed by using raw materials such as graphene oxide fiber, alginate fiber, polyurethane biguanide, imidazole salt, imidazole ketone salt, saccharin salt and alginate through copolymerization and ion exchange reactions.

Benefits of technology

It significantly improves antibacterial effect, mechanical properties and resistance to damp heat aging, extends service life, and improves feel and resistance to compression set.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004793149970000071
    Figure BDA0004793149970000071
Patent Text Reader

Abstract

The invention provides an antibacterial fiber sponge material and a preparation method thereof, and relates to the technical field of sponge materials, comprising raw materials: graphene oxide fiber, alginate fiber, polyethersulfone type hyperbranched epoxy resin with epoxy end groups, polyaminopropyl biguanide, 2,4-diamino-6-diallylamino-1,3,5-triazine, 1-allyl-3-vinylimidazole chloride, bis(1-vinylimidazole-2-)ketone, 2-methyl-N-[2-(2-oxygen-1-imidazolidinyl)ethyl]-2-acrylamide, 3-(1,1-difluoro-2-propylene-1-yl)-2(1H)-quinoxalinone, polymerizable ester, initiator, foaming agent, saccharin sodium, and sodium alginate. The material has significant antibacterial effect, good mechanical properties, good resistance to wet heat aging, strong resistance to compression permanent deformation, good hand feel, and long service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sponge materials, and in particular to an antibacterial fiber sponge material and a preparation method thereof. Background Art

[0002] Sponge is a porous material with good water absorption performance. It has good moisture absorption, thermal insulation, sound absorption and shock absorption, flame retardant and anti-static properties. It is widely used in the production and protection of products in various fields such as automobiles, furniture, daily necessities, underwear, etc. With the improvement of people's living standards and the rapid development of the economy, the requirements for sponge materials are no longer just to meet the basic functions of moisture absorption, thermal insulation, sound absorption and shock absorption, flame retardant and anti-static. People are now more concerned about its safety and environmental protection.

[0003] Since sponge materials have good hygroscopicity, they can easily absorb moisture in the environment and breed various bacteria inside. Especially in places with warm and humid climates, the hot and humid interior of sponge materials provides a breeding ground for bacteria such as mold, which not only brings inconvenience to use, but also poses a hidden danger to people's health. In order to give sponge materials antibacterial function, the current common practice is to add antibacterial agents into them. However, the compatibility between existing antibacterial agents and sponge material substrates is poor, and the antibacterial stability is insufficient after long-term use, and the antibacterial effect still needs to be further improved. In addition, the antibacterial sponge materials on the market have more or less technical defects such as limited mechanical properties, poor hand feel, insufficient stability, easy deformation, short service life, and insufficient antibacterial broad-spectrum.

[0004] In order to solve the above problems, the Chinese invention patent with the authorization announcement number CN117186347B discloses a modified bamboo fiber sponge, which includes, by weight, 35-55 parts of modified polyisocyanate, 95-110 parts of polyol, 10-20 parts of modified bamboo fiber, 1.5-2.5 parts of foaming agent, 0.6-1.2 parts of silicone oil and 0.3-0.5 parts of catalyst. The invention prepares a modified bamboo fiber sponge, which uses modified polyisocyanate and polyol as reaction raw materials and modified bamboo fiber as modification raw material. The prepared modified bamboo fiber sponge not only enhances the antibacterial performance of the sponge, but also improves the basic performance of traditional bamboo fiber sponge, such as hand feel, strength, elasticity and aging resistance. However, its resistance to wet heat aging and deformation resistance still need to be further improved.

[0005] Therefore, the development of an antibacterial fiber sponge material with significant antibacterial effect, good mechanical properties, good resistance to moisture and heat aging, strong resistance to compression permanent deformation, good hand feel and long service life and its preparation method meet market demand, have broad market value and application prospects, and are of great significance to promoting the development of the sponge material field. Summary of the invention

[0006] In view of the above problems, the object of the present invention is to provide an antibacterial fiber sponge material with significant antibacterial effect, good mechanical properties, good resistance to moisture and heat aging, strong resistance to permanent compression deformation, good hand feel and long service life, and a preparation method thereof.

[0007] In order to achieve the above-mentioned purpose, the technical scheme adopted by the present invention is: an antibacterial fiber sponge material is made of the following raw materials in parts by weight: 10-20 parts of graphene oxide fiber, 3-5 parts of alginate fiber, 15-25 parts of polyethersulfone type hyperbranched epoxy resin with epoxy end groups, 3-5 parts of polyaminopropyl biguanide, 2-4 parts of 2,4-diamino-6-diallylamino-1,3,5-triazine, 1-allyl-3-vinyl imidazole 5-8 parts of chloride salt, 1-3 parts of bis(1-vinyl imidazole-2-)ketone, 2-4 parts of 2-methyl-N-[2-(2-oxo-1-imidazolidinyl)ethyl]-2-acrylamide, 1-3 parts of 3-(1,1-difluoro-2-propene-1-yl)-2(1H)-quinoxalinone, 30-40 parts of polymerizable ester, 0.5-0.8 parts of initiator, 2-4 parts of foaming agent, 1-2 parts of saccharin sodium, and 0.3-0.6 parts of sodium alginate.

[0008] Preferably, the foaming agent is a mixture of foaming agent TSH and N,N'-dinitroso-N,N'-dimethylterephthalamide in a mass ratio of 1:(1-2).

[0009] Preferably, the initiator is dicumyl peroxide.

[0010] Preferably, the polymerizable ester is a mixture of butyl acrylate, hydroxyethyl acrylate and 2-methoxyethyl acrylate in a mass ratio of 1:(0.8-1.2):(1-2).

[0011] Preferably, the CAS number of the polyaminopropyl biguanide is 133029-32-0, the product number is P914934-500g, and it is provided by McLean.

[0012] Preferably, there is no special requirement for the source of the polyethersulfone type hyperbranched epoxy resin with epoxy terminal groups. In one embodiment of the present invention, the polyethersulfone type hyperbranched epoxy resin with epoxy terminal groups is prepared according to the method of Chinese invention patent implementation case 18 with authorization announcement number CN104311832B.

[0013] Preferably, the alginate fiber has a fineness of 0.8-1.1 dtex and a length of 5-15 mm.

[0014] Preferably, the graphene oxide fiber has a fineness of 0.3-0.8 dtex and a length of 6-20 mm.

[0015] Another object of the present invention is to provide a method for preparing the antibacterial fiber sponge material, comprising the following steps:

[0016] Step S1, after the other raw materials except sodium saccharin and sodium alginate are dispersed uniformly by weight, the raw materials are added into a mold, sealed and foamed at 110-120° C. for 8-20 minutes, and demolded to obtain a primary fiber sponge material;

[0017] Step S2, soaking the raw fiber sponge material prepared in step S1 in a mixed aqueous solution of sodium saccharin and sodium alginate at 50-60° C. for 15-25 hours, taking it out, washing it with water, and drying it in sequence to obtain the antibacterial fiber sponge material.

[0018] Preferably, the mass ratio of saccharin sodium to water in the mixed aqueous solution of saccharin sodium and sodium alginate is 1:(6-10).

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] (1) The preparation method of the antibacterial fiber sponge material disclosed in the present invention has simple process, convenient operation and control, high preparation efficiency and finished product qualification rate, low dependence on equipment, low energy consumption, suitable for continuous large-scale production, and has high promotion and application value.

[0021] (2) The antibacterial fiber sponge material disclosed in the present invention is made of the following raw materials in parts by weight: 10-20 parts of graphene oxide fiber, 3-5 parts of alginate fiber, 15-25 parts of polyethersulfone type hyperbranched epoxy resin with epoxy end groups, 3-5 parts of polyaminopropyl biguanide, 2-4 parts of 2,4-diamino-6-diallylamino-1,3,5-triazine, 5-8 parts of 1-allyl-3-vinyl imidazole chloride, 1-3 parts of (1-vinyl imidazole-2-) ketone, 2-4 parts of 2-methyl-N-[2-(2-oxy-1-imidazolidinyl)ethyl]-2-acrylamide, 1-3 parts of 3-(1,1-difluoro-2-propylene-1-yl)-2(1H)-quinoxalinone, 30-40 parts of polymerizable ester, 0.5-0.8 parts of initiator, 2-4 parts of foaming agent, 1-2 parts of sodium saccharin, and 0.3-0.6 parts of sodium alginate. Through the mutual cooperation and joint action of various raw materials, the prepared fiber sponge material has significant antibacterial effect, good mechanical properties, good resistance to moisture and heat aging, strong resistance to compression permanent deformation, good hand feel, and long service life. The added graphene oxide fiber and alginate fiber surfaces contain more oxygen-containing groups, and have good compatibility with other raw materials, thereby improving the performance stability of the product and extending its service life. The synergistic effect of graphene oxide fiber, alginate fiber, polyaminopropyl biguanide, imidazole salt, imidazolide salt, saccharin salt and alginate can give the product excellent antibacterial effect, making it have better antibacterial spectrum and stability, and extending the service life of the product.

[0022] (3) The antibacterial fiber sponge material disclosed in the present invention comprises monomers containing unsaturated olefinic bonds which can undergo copolymerization reaction under the action of an initiator, raw materials containing epoxy groups can undergo epoxy ring-opening reaction with raw materials containing amino groups, and sodium saccharin and sodium alginate can undergo ion exchange reaction with 1-allyl-3-vinyl imidazolium chloride, so that a variety of interpenetrating network structures exist in the molecular structure of the prepared sponge material product, which can not only improve the performance stability of the product, but also help to improve the mechanical properties, moisture-heat aging resistance and compression permanent deformation resistance, thereby extending its service life.

[0023] (4) The antibacterial fiber sponge material disclosed in the present invention has a uniform pore size, a high porosity, good hand feel and mechanical properties, and good resistance to permanent deformation and moisture-heat aging through the reasonable selection of raw material ratios, foaming agents and preparation process parameters, thereby effectively improving the use effect of the sponge material and extending its service life. DETAILED DESCRIPTION

[0024] In order to enable those skilled in the art to better understand the technical solution of the present invention, the product of the present invention is further described in detail below in conjunction with embodiments.

[0025] Example 1

[0026] An antibacterial fiber sponge material is prepared from the following raw materials in parts by weight: 10 parts of graphene oxide fiber, 3 parts of alginate fiber, 15 parts of polyethersulfone type hyperbranched epoxy resin with epoxy end groups, 3 parts of polyaminopropyl biguanide, 2 parts of 2,4-diamino-6-diallylamino-1,3,5-triazine, 5 parts of 1-allyl-3-vinylimidazole chloride, 1 part of bis(1-vinylimidazole-2-)ketone, 2 parts of 2-methyl-N-[2-(2-oxy-1-imidazolidinyl)ethyl]-2-acrylamide, 1 part of 3-(1,1-difluoro-2-propylene-1-yl)-2(1H)-quinoxalinone, 30 parts of polymerizable ester, 0.5 parts of initiator, 2 parts of foaming agent, 1 part of saccharin sodium and 0.3 parts of sodium alginate.

[0027] The foaming agent is a mixture of foaming agent TSH and N,N'-dinitroso-N,N'-dimethylterephthalamide in a mass ratio of 1:1; the initiator is dicumyl peroxide; and the polymerizable ester is a mixture of butyl acrylate, hydroxyethyl acrylate, and 2-methoxyethyl acrylate in a mass ratio of 1:0.8:1.

[0028] The CAS number of the polyaminopropyl biguanide is 133029-32-0, the product number is P914934-500g, and it is provided by McLean; the polyethersulfone type hyperbranched epoxy resin with epoxy end groups is prepared according to the method of Chinese invention patent implementation case 18 with authorization announcement number CN104311832B.

[0029] The alginate fiber has a fineness of 0.8 dtex and a length of 5 mm; the graphene oxide fiber has a fineness of 0.3 dtex and a length of 6 mm.

[0030] A method for preparing the antibacterial fiber sponge material comprises the following steps:

[0031] Step S1, after the other raw materials except sodium saccharin and sodium alginate are dispersed uniformly by weight, the raw materials are added into a mold, sealed and foamed at 110° C. for 8 minutes, and demolded to obtain a primary fiber sponge material;

[0032] Step S2, soaking the primary fiber sponge material prepared in step S1 in a mixed aqueous solution of sodium saccharin and sodium alginate at 50° C. for 15 hours, taking it out, washing it with water, and drying it in sequence to obtain an antibacterial fiber sponge material; the mass ratio of sodium saccharin to water in the mixed aqueous solution of sodium saccharin and sodium alginate is 1:6.

[0033] Example 2

[0034] An antibacterial fiber sponge material is prepared from the following raw materials in parts by weight: 13 parts of graphene oxide fiber, 3.5 parts of alginate fiber, 17 parts of polyethersulfone type hyperbranched epoxy resin with epoxy end groups, 3.5 parts of polyaminopropyl biguanide, 2.5 parts of 2,4-diamino-6-diallylamino-1,3,5-triazine, 6 parts of 1-allyl-3-vinylimidazole chloride, 1.5 parts of bis(1-vinylimidazole-2-)ketone, 2.5 parts of 2-methyl-N-[2-(2-oxy-1-imidazolidinyl)ethyl]-2-acrylamide, 1.5 parts of 3-(1,1-difluoro-2-propylene-1-yl)-2(1H)-quinoxalinone, 33 parts of polymerizable ester, 0.6 parts of initiator, 2.5 parts of foaming agent, 1.2 parts of saccharin sodium and 0.4 parts of sodium alginate.

[0035] The foaming agent is a mixture of foaming agent TSH and N,N'-dinitroso-N,N'-dimethylterephthalamide in a mass ratio of 1:1.3; the initiator is dicumyl peroxide; and the polymerizable ester is a mixture of butyl acrylate, hydroxyethyl acrylate, and 2-methoxyethyl acrylate in a mass ratio of 1:0.9:1.2.

[0036] The CAS number of the polyaminopropyl biguanide is 133029-32-0, the product number is P914934-500g, and it is provided by McLean; the polyethersulfone type hyperbranched epoxy resin with epoxy end groups is made according to the method of Chinese invention patent implementation case 18 with authorization announcement number CN104311832B; the fineness of the alginate fiber is 0.9 dtex and the length is 8 mm; the fineness of the graphene oxide fiber is 0.4 dtex and the length is 10 mm.

[0037] A method for preparing the antibacterial fiber sponge material comprises the following steps:

[0038] Step S1, after the other raw materials except sodium saccharin and sodium alginate are dispersed uniformly by weight, the raw materials are added into a mold, sealed and foamed at 113° C. for 12 minutes, and demolded to obtain a primary fiber sponge material;

[0039] Step S2, soaking the primary fiber sponge material prepared in step S1 in a mixed aqueous solution of sodium saccharin and sodium alginate at 53° C. for 18 hours, taking it out, washing it with water, and drying it in sequence to obtain an antibacterial fiber sponge material; the mass ratio of sodium saccharin to water in the mixed aqueous solution of sodium saccharin and sodium alginate is 1:7.

[0040] Example 3

[0041] An antibacterial fiber sponge material is prepared from the following raw materials in parts by weight: 15 parts of graphene oxide fiber, 4 parts of alginate fiber, 20 parts of polyethersulfone type hyperbranched epoxy resin with epoxy end groups, 4 parts of polyaminopropyl biguanide, 3 parts of 2,4-diamino-6-diallylamino-1,3,5-triazine, 6.5 parts of 1-allyl-3-vinylimidazole chloride, 2 parts of bis(1-vinylimidazole-2-)ketone, 3 parts of 2-methyl-N-[2-(2-oxy-1-imidazolidinyl)ethyl]-2-acrylamide, 2 parts of 3-(1,1-difluoro-2-propylene-1-yl)-2(1H)-quinoxalinone, 35 parts of polymerizable ester, 0.65 parts of initiator, 3 parts of foaming agent, 1.5 parts of saccharin sodium and 0.45 parts of sodium alginate.

[0042] The foaming agent is a mixture of foaming agent TSH and N,N'-dinitroso-N,N'-dimethylterephthalamide in a mass ratio of 1:1.5; the initiator is dicumyl peroxide; and the polymerizable ester is a mixture of butyl acrylate, hydroxyethyl acrylate, and 2-methoxyethyl acrylate in a mass ratio of 1:1:1.5.

[0043] The CAS number of the polyaminopropyl biguanide is 133029-32-0, the product number is P914934-500g, and it is provided by McLean; the polyethersulfone type hyperbranched epoxy resin with epoxy end groups is made according to the method of Chinese invention patent implementation case 18 with authorization announcement number CN104311832B; the fineness of the alginate fiber is 1 dtex and the length is 10 mm; the fineness of the graphene oxide fiber is 0.5 dtex and the length is 12 mm.

[0044] A method for preparing the antibacterial fiber sponge material comprises the following steps:

[0045] Step S1, after the other raw materials except sodium saccharin and sodium alginate are dispersed uniformly by weight, the raw materials are added into a mold, sealed and foamed at 115° C. for 14 minutes, and demolded to obtain a primary fiber sponge material;

[0046] Step S2, soaking the primary fiber sponge material prepared in step S1 in a mixed aqueous solution of sodium saccharin and sodium alginate at 55° C. for 20 hours, taking it out, washing it with water, and drying it in sequence to obtain an antibacterial fiber sponge material; the mass ratio of sodium saccharin to water in the mixed aqueous solution of sodium saccharin and sodium alginate is 1:8.

[0047] Example 4

[0048] An antibacterial fiber sponge material is prepared from the following raw materials in parts by weight: 18 parts of graphene oxide fiber, 4.5 parts of alginate fiber, 23 parts of polyethersulfone type hyperbranched epoxy resin with epoxy end groups, 4.5 parts of polyaminopropyl biguanide, 3.5 parts of 2,4-diamino-6-diallylamino-1,3,5-triazine, 7.5 parts of 1-allyl-3-vinylimidazole chloride, 2.5 parts of bis(1-vinylimidazole-2-)ketone, 3.5 parts of 2-methyl-N-[2-(2-oxy-1-imidazolidinyl)ethyl]-2-acrylamide, 2.5 parts of 3-(1,1-difluoro-2-propylene-1-yl)-2(1H)-quinoxalinone, 38 parts of polymerizable ester, 0.75 parts of initiator, 3.5 parts of foaming agent, 1.8 parts of saccharin sodium and 0.55 parts of sodium alginate.

[0049] The foaming agent is a mixture of foaming agent TSH and N,N'-dinitroso-N,N'-dimethylterephthalamide in a mass ratio of 1:1.8; the initiator is dicumyl peroxide; and the polymerizable ester is a mixture of butyl acrylate, hydroxyethyl acrylate, and 2-methoxyethyl acrylate in a mass ratio of 1:1.1:1.9.

[0050] The CAS number of the polyaminopropyl biguanide is 133029-32-0, the product number is P914934-500g, and it is provided by McLean; the polyethersulfone type hyperbranched epoxy resin with epoxy end groups is made according to the method of Chinese invention patent implementation case 18 with authorization announcement number CN104311832B; the fineness of the alginate fiber is 1 dtex and the length is 13 mm; the fineness of the graphene oxide fiber is 0.7 dtex and the length is 18 mm.

[0051] A method for preparing the antibacterial fiber sponge material comprises the following steps:

[0052] Step S1, after the other raw materials except sodium saccharin and sodium alginate are dispersed uniformly by weight, the mixture is added into a mold, and the mixture is sealed and foamed at 118° C. for 18 minutes, and the mold is demoulded to obtain a primary fiber sponge material;

[0053] Step S2, soaking the primary fiber sponge material prepared in step S1 in a mixed aqueous solution of sodium saccharin and sodium alginate at 58° C. for 23 hours, taking it out, washing it with water, and drying it in sequence to obtain an antibacterial fiber sponge material; the mass ratio of sodium saccharin to water in the mixed aqueous solution of sodium saccharin and sodium alginate is 1:9.5.

[0054] Example 5

[0055] An antibacterial fiber sponge material is prepared from the following raw materials in parts by weight: 20 parts of graphene oxide fiber, 5 parts of alginate fiber, 25 parts of polyethersulfone type hyperbranched epoxy resin with epoxy end groups, 5 parts of polyaminopropyl biguanide, 4 parts of 2,4-diamino-6-diallylamino-1,3,5-triazine, 8 parts of 1-allyl-3-vinylimidazole chloride, 3 parts of bis(1-vinylimidazole-2-)ketone, 4 parts of 2-methyl-N-[2-(2-oxy-1-imidazolidinyl)ethyl]-2-acrylamide, 3 parts of 3-(1,1-difluoro-2-propylene-1-yl)-2(1H)-quinoxalinone, 40 parts of polymerizable ester, 0.8 parts of initiator, 4 parts of foaming agent, 2 parts of saccharin sodium and 0.6 parts of sodium alginate.

[0056] The foaming agent is a mixture of foaming agent TSH and N,N'-dinitroso-N,N'-dimethylterephthalamide in a mass ratio of 1:2; the initiator is diisopropyl peroxide; the polymerizable ester is a mixture of butyl acrylate, hydroxyethyl acrylate and 2-methoxyethyl acrylate in a mass ratio of 1:1.2:2; the CAS number of the polyaminopropyl biguanide is 133029-32-0, the product number is P914934-500g, and it is provided by McLean.

[0057] The polyethersulfone type hyperbranched epoxy resin with epoxy end groups is made according to the method of Chinese invention patent implementation case 18 with authorization announcement number CN104311832B; the fineness of the alginate fiber is 1.1 dtex and the length is 15 mm; the fineness of the graphene oxide fiber is 0.8 dtex and the length is 20 mm.

[0058] A method for preparing the antibacterial fiber sponge material comprises the following steps:

[0059] Step S1, after the other raw materials except sodium saccharin and sodium alginate are dispersed uniformly by weight, the mixture is added into a mold, and the mixture is sealed and foamed at 120° C. for 20 minutes, and the mold is demoulded to obtain a primary fiber sponge material;

[0060] Step S2, soaking the primary fiber sponge material prepared in step S1 in a mixed aqueous solution of sodium saccharin and sodium alginate at 60° C. for 25 hours, taking it out, washing it with water, and drying it in sequence to obtain an antibacterial fiber sponge material; the mass ratio of sodium saccharin to water in the mixed aqueous solution of sodium saccharin and sodium alginate is 1:10.

[0061] Comparative Example 1

[0062] An antibacterial fiber sponge material is substantially the same as Example 1, except that polyaminopropyl biguanide and 3-(1,1-difluoro-2-propylene-1-yl)-2(1H)-quinoxalinone are not added.

[0063] Comparative Example 2

[0064] An antibacterial fiber sponge material is substantially the same as Example 1, except that 2-methyl-N-[2-(2-oxo-1-imidazolidinyl)ethyl]-2-acrylamide and saccharin sodium are not added.

[0065] In order to further illustrate the unexpected positive technical effects achieved by the products of each embodiment of the present invention, relevant performance tests were conducted on the antibacterial fiber sponge materials prepared in each example. The test results are shown in Table 1. The test methods are as follows: the feel is the artificial touch feeling, and the actual touch evaluation is performed by an evaluation team composed of ten people; the tensile strength is tested with reference to the method of standard ISO 1798-2008; the compression permanent deformation is tested with reference to the method of standard ISO 1856-2007; the conditions for wet heat aging are: temperature 80°C, humidity 95%, and aging for 120h; the antibacterial property, the test includes Escherichia coli and Staphylococcus aureus, and the test standard refers to GB / T20944.3-2008.

[0066] Table 1

[0067]

[0068] As can be seen from Table 1, the antibacterial fiber sponge material disclosed in the embodiment of the present invention has better mechanical properties, hand feel, antibacterial property, resistance to permanent deformation and resistance to moist heat aging than the comparative example product. The addition of polyaminopropyl biguanide, 3-(1,1-difluoro-2-propene-1-yl)-2(1H)-quinoxalinone, 2-methyl-N-[2-(2-oxy-1-imidazolidinyl)ethyl]-2-acrylamide and saccharin sodium is beneficial to improving the above properties.

[0069] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any ordinary technician in the industry can smoothly implement the present invention as described above. However, any technician familiar with the profession can make some changes, modifications and evolutions of the technical content disclosed above without departing from the scope of the technical solution of the present invention, which are all equivalent embodiments of the present invention. At the same time, any changes, modifications and evolutions of any equivalent changes made to the above embodiments based on the essential technology of the present invention are still within the protection scope of the technical solution of the present invention.

Claims

1. An antibacterial fiber sponge material, It is characterized in that The invention is prepared from the following raw materials in parts by weight: 10-20 parts of graphene oxide fiber, 3-5 parts of alginate fiber, 15-25 parts of polyethersulfone type hyperbranched epoxy resin with epoxy end groups, 3-5 parts of polyaminopropyl biguanide, 2-4 parts of 2,4-diamino-6-diallylamino-1,3,5-triazine, 5-8 parts of 1-allyl-3-vinylimidazole chloride, 1-3 parts of bis(1-vinylimidazole-2-)ketone, 2-4 parts of 2-methyl-N-[2-(2-oxy-1-imidazolidinyl)ethyl]-2-acrylamide, 1-3 parts of 3-(1,1-difluoro-2-propylene-1-yl)-2(1H)-quinoxalinone, 30-40 parts of polymerizable ester, 0.5-0.8 parts of initiator, 2-4 parts of foaming agent, 1-2 parts of saccharin sodium, and 0.3-0.6 parts of sodium alginate; The method for preparing the antibacterial fiber sponge material comprises the following steps: Step S1, after the other raw materials except sodium saccharin and sodium alginate are dispersed uniformly by weight, the raw materials are added into a mold, sealed and foamed at 110-120° C. for 8-20 minutes, and demolded to obtain a primary fiber sponge material; Step S2, soaking the raw fiber sponge material prepared in step S1 in a mixed aqueous solution of sodium saccharin and sodium alginate at 50-60° C. for 15-25 hours, taking it out, washing it with water, and drying it in sequence to obtain an antibacterial fiber sponge material; the mass ratio of sodium saccharin to water in the mixed aqueous solution of sodium saccharin and sodium alginate is 1:(6-10).

2. The antibacterial fiber sponge material according to claim 1, It is characterized in that The foaming agent is a mixture of foaming agent TSH and N,N'-dinitroso-N,N'-dimethylterephthalamide in a mass ratio of 1:(1-2).

3. The antibacterial fiber sponge material according to claim 1, It is characterized in that The initiator is dicumyl peroxide.

4. The antibacterial fiber sponge material according to claim 1, It is characterized in that The polymerizable ester is a mixture of butyl acrylate, hydroxyethyl acrylate and 2-methoxyethyl acrylate in a mass ratio of 1:(0.8-1.2):(1-2).

5. The antibacterial fiber sponge material according to claim 1, It is characterized in that The alginate fiber has a fineness of 0.8-1.1 dtex and a length of 5-15 mm.

6. The antibacterial fiber sponge material according to claim 1, It is characterized in that The graphene oxide fiber has a fineness of 0.3-0.8 dtex and a length of 6-20 mm.

Citation Information

Patent Citations

  • Preparation method of a polyethersulfone-based hyperbranched epoxy resin and its application in toughening linear epoxy resin

    CN104311832B

  • A modified bamboo fiber sponge and preparation method thereof

    CN117186347B

  • Preparation method of polyethersulfone type hyper branched epoxy resin and application in toughening of linear epoxy resin

    CN104311832A

  • Preparing method of cleaning sponge with high pollutant receiving ability

    CN107033392A

  • A method for preparing a reinforced polymethacrylimide foam composite material