Composite metallocene polyethylene composition for packaging film, composite metallocene polyethylene and preparation method of composite metallocene polyethylene composition

By mixing two different metallocene polyethylenes in a high-temperature mixer, combining antioxidants and dispersants, the problem of poor processing and mechanical properties of metallocene polyethylene in the manufacturing of polyethylene packaging film is solved, and a single Raw materials replace a variety of raw materials, simplify processes and improve film performance.

CN118994773AInactive Publication Date: 2024-11-22XINJIANG DUSHANZI PETROCHEMICAL CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411489360.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-24
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

There is a contradiction between the processing performance and mechanical properties of existing metallocene polyethylene in the manufacturing of polyethylene packaging films, resulting in poor performance of film products and physical blending of multiple polyethylene raw materials, resulting in uneven cutting and complex process. .

Method used

Using two different metallocene polyethylene compositions, the mixing is carried out in a high-temperature mixer with the assistance of antioxidants and dispersants, the door opening and granular water temperature are adjusted to synthesize both processing and mechanical properties. Composite metallocene polyethylene.

Benefits of technology

A single raw material replaces multiple raw materials, improves the quality of films, simplifies production processes, improves the melt mass flow rate, tensile yield stress, dart impact strength and tensile fracture nominal strain of metallocene polyethylene, and reduces production Difficulty and cost.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a composite metallocene polyethylene composition for a packaging film, composite metallocene polyethylene and a preparation method of the composite metallocene polyethylene composition. The composition is prepared from the following raw materials in parts by weight: 50 to 70 parts of first metallocene polyethylene, 30 to 50 parts of second metallocene polyethylene, 0.0002 to 0.002 part of an antioxidant and 0.0002 to 0.002 part of a dispersing agent. The preparation method takes the composition as a raw material and comprises the following steps: mixing first metallocene polyethylene and second metallocene polyethylene to obtain a metallocene polyethylene mixture; mixing an antioxidant and a dispersing agent to obtain a composite additive; and mixing the metallocene polyethylene mixture and the composite additive to obtain the composite metallocene polyethylene. The composite metallocene polyethylene has both processability and mechanical properties, is simple in process and low in cost, and can replace other raw material components conventionally applied to polyethylene packaging films.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of petrochemical industry and relates to a composite metallocene polyethylene composition for packaging film and a composite metallocene polyethylene and a preparation method thereof. Background Art

[0002] Metallocene polyethylene is a polyethylene resin polymerized by a catalyst consisting of metallocene organic compounds and co-catalysts. Its main suppliers include DOW Chemicals, ExxonMobil, etc., and the grades it produces are specialized. Currently, more than 90% of metallocene polyethylene on the market are used in the film field, but due to the characteristics of the catalyst, the performance characteristics of metallocene polyethylene currently mainly include the following two aspects: ① Excellent processing performance, but poor mechanical properties; ② Excellent mechanical properties, but poor processing performance. Therefore, metallocene polyethylene often has bottlenecks in film manufacturing.

[0003] In the manufacturing process of polyethylene packaging film, it is necessary to physically blend the polyethylene raw materials (ordinary linear low-density polyethylene, i.e. LLDPE; low-density polyethylene, i.e. LDPE) with different required properties for a certain period of time by using large agitators or manual stirring, and then process the required polyethylene packaging film. However, this method requires physical mixing of different polyethylene raw materials, which requires many types of raw materials, and it is impossible to mix several metallocene polyethylenes from the molecular structure, resulting in uneven raw material feeding and poor performance of the film products during the use of the obtained polyethylene packaging film. For example, there are often too many fish eyes in the film products, resulting in unqualified film products.

[0004] Therefore, it is necessary to develop a metallocene polyethylene that can take into account both processing performance and mechanical properties for use in the field of polyethylene packaging films. When the metallocene polyethylene is used to prepare polyethylene packaging films, a small amount of polyethylene raw material can be used to replace many conventional types of polyethylene raw materials, ultimately achieving the purpose of improving film quality and reducing production processes. Summary of the invention

[0005] In order to solve the problems existing in the prior art, the present invention provides a composite metallocene polyethylene composition for packaging film and a composite metallocene polyethylene and a preparation method thereof, wherein a metallocene polyethylene product having excellent processing performance but poor mechanical properties is mixed with a metallocene polyethylene product having poor processing performance but excellent mechanical properties, and a reasonable mixing method is adopted with the assistance of an antioxidant and a dispersant to obtain a metallocene polyethylene product having both processing performance and mechanical properties.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions.

[0007] In a first aspect, the present invention provides a composite metallocene polyethylene composition for packaging film, wherein the composite metallocene polyethylene composition comprises the following raw materials in parts by weight: 50 to 70 parts of the first metallocene polyethylene, 30 to 50 parts of the second metallocene polyethylene, 0.0002 to 0.002 parts of antioxidant, and 0.0002 to 0.002 parts of dispersant.

[0008] In the composite metallocene polyethylene composition, the mechanical properties of the first metallocene polyethylene are better than those of the second metallocene polyethylene, and the processing properties of the second metallocene polyethylene are better than those of the first metallocene polyethylene.

[0009] The composite metallocene polyethylene composition, wherein the first metallocene polyethylene is a polymer obtained by copolymerizing ethylene with 1-hexene or 1-butene in the presence of a first metallocene catalyst, has a molecular weight distribution index of 2 to 3 and a density of 0.916 g / cm 3 Up to 0.935 g / cm 3 .

[0010] The composite metallocene polyethylene composition, wherein the critical shear rate of the first metallocene polyethylene is 300 s -1 .

[0011] The composite metallocene polyethylene composition, wherein the second metallocene polyethylene is a polymer obtained by copolymerizing ethylene with 1-hexene or 1-butene in the presence of a second metallocene catalyst, has a molecular weight distribution width index of 3 to 4, and a density of 0.916 g / cm 3 Up to 0.935 g / cm 3 .

[0012] In the present invention, the first metallocene polyethylene has excellent mechanical properties but poor processing properties, and the second metallocene polyethylene has excellent processing properties but poor mechanical properties.

[0013] The critical shear rate of the second metallocene polyethylene composition is 650 s -1 .

[0014] In the composite metallocene polyethylene composition, the melt mass flow rate (MFR, also called melt flow index or melt index) of the first metallocene polyethylene is 0.5 g / l0 min to 3.5 g / l0 min.

[0015] In the composite metallocene polyethylene composition, the melt mass flow rate (MFR) of the second metallocene polyethylene is 0.5 g / l0 min to 3.5 g / l0 min.

[0016] In the composite metallocene polyethylene composition, the first metallocene catalyst and the second metallocene catalyst are different metallocene catalysts.

[0017] In the composite metallocene polyethylene composition, the antioxidant comprises at least one of antioxidant 1010, antioxidant 1076 and antioxidant 168.

[0018] In the composite metallocene polyethylene composition, the dispersant comprises at least one of polyethylene wax and polyethylene glycol.

[0019] In the present invention, the first metallocene polyethylene has excellent mechanical properties, but poor processing properties; the second metallocene polyethylene has excellent processing properties, but poor mechanical properties. The present invention composites the first metallocene polyethylene and the second metallocene polyethylene together, striving to combine the excellent properties of the two into one, taking advantage of their strengths and avoiding their weaknesses, and obtaining a composite metallocene polyethylene material for packaging film that has both excellent processing properties and mechanical properties. Compared with the use of a single metallocene polyethylene with a wide molecular weight distribution, it is easier to regulate the properties of the required composite metallocene polyethylene, and the operation method is simpler.

[0020] In addition, since the first metallocene polyethylene and the second metallocene polyethylene are both metallocene polyethylenes, the miscibility of the two is better than that of conventional polyethylene and metallocene polyethylene, and thus they are easy to mix and knead to obtain a uniform composite metallocene polyethylene material, which is conducive to obtaining a metallocene polyethylene product with excellent performance. In the present invention, the two metallocene polyethylenes are mixed, combined with a small amount of antioxidant (to prevent the raw materials or products from being oxidized) and a dispersant (to facilitate the uniform distribution of each raw material in the mixed system) to obtain a composite metallocene polyethylene with excellent processing properties and mechanical properties for use in the field of polyethylene packaging films, the types of raw materials used are small, the amount of antioxidant and dispersant used is small, and the production process is simple.

[0021] In a second aspect, the present invention provides a method for preparing a composite metallocene polyethylene for packaging film, using any of the composite metallocene polyethylene compositions for packaging film as a raw material, and the preparation method comprises the following steps: 1) obtaining the first metallocene polyethylene and storing it for future use; 2) mixing the first metallocene polyethylene with the second metallocene polyethylene to obtain a metallocene polyethylene mixture; 3) Mixing the antioxidant and the dispersant to obtain a composite additive; 4) kneading the metallocene polyethylene mixture and the composite additive, and then cooling and pelletizing to obtain the composite metallocene polyethylene for packaging film (also referred to as polyethylene film material or polyethylene film material).

[0022] In the method for preparing the composite metallocene polyethylene for packaging film, in the step 1), the first metallocene polyethylene is sealed with nitrogen during storage.

[0023] In the present invention, nitrogen is used to seal the first metallocene polyethylene to prevent the first metallocene polyethylene from being oxidized during storage.

[0024] In the method for preparing the composite metallocene polyethylene for packaging film, in the step 1), the obtained first metallocene polyethylene is placed in a buffer silo for storage for later use.

[0025] In the method for preparing the composite metallocene polyethylene for packaging film, in the step 2), the first metallocene polyethylene is mixed with the second metallocene polyethylene being produced in a rotary feeder (eg, a large spiral rotary feeder).

[0026] In the method for preparing the composite metallocene polyethylene for packaging film, in the step 4), the mixing is performed using a mixer.

[0027] In the method for preparing the composite metallocene polyethylene for packaging film, in the step 4), during the mixing process, the temperature of the extruder barrel is 250°C to 280°C.

[0028] In the present invention, the two mixed metallocene polyethylenes and the composite additives are added to a mixer for mixing. Under the action of high temperature, the two metallocene polyethylenes and related materials are melted, and then the molecular chain segments of the two metallocene polyethylenes are disentangled and moved under the action of heat; under the action of screw stirring, the molecular chain segments of the two metallocene polyethylenes are rearranged to obtain a composite metallocene polyethylene resin with a new molecular chain structure. During the mixing process, if the temperature is too high, the metallocene polyethylene material will be degraded or cross-linked, and if the temperature is too low, it will be unfavorable for processing the raw materials.

[0029] In the method for preparing the composite metallocene polyethylene for packaging film, in the step 4), during the mixing process, the door opening is adjusted to 15% to 28%.

[0030] In the present invention, the performance of the mixed product is controlled by controlling the opening of the regulating gate during the mixing process. The lower the regulating gate, the better the mixing effect of the materials, that is, the easier it is to mix evenly. However, too low an opening of the gate may lead to degradation or cross-linking of the materials.

[0031] In the method for preparing the composite metallocene polyethylene for packaging film, in the step 4), the temperature of pelletizing water used during pelletizing is less than 40°C.

[0032] In the present invention, the opening of the mixer door is lowered to allow various materials to fully stay and mix. After being cooled by pelletizing water and the cutter rotates, the mixed material extruded from the mixer is cooled in a very short time, wherein the two metallocene polyethylene molecular segments are rearranged and crystallized and solidified under the rapid cooling of pelletizing water.

[0033] In a third aspect, the present invention provides a composite metallocene polyethylene for packaging film, wherein the composite metallocene polyethylene for packaging film is prepared by any of the above-mentioned methods for preparing the composite metallocene polyethylene for packaging film.

[0034] In the present invention, the molecular chain segments of the composite metallocene polyethylene for packaging film include metallocene polyethylene with a molecular weight distribution of 2 to 3 and poor processing performance but excellent mechanical properties, and metallocene polyethylene with a molecular weight distribution of 3 to 4 and poor mechanical properties but excellent processing performance. Under the action of a mixer, the molecular chain segments of the two metallocene polyethylenes are rearranged, crystallized and solidified, thereby forming a metallocene polyethylene with both processing performance and mechanical properties.

[0035] In the present invention, the composite metallocene polyethylene for packaging film has the following characteristics: Melt mass flow rate is 0.5 g / 10 min to 3.5 g / 10 min, density is 0.916 g / cm 3 Up to 0.935g / cm 3 , tensile yield stress ≥18 MPa, dart impact strength ≥900 g, tensile fracture nominal strain ≥700%, critical shear rate>600 s -1 , yellow index ≤0.

[0036] The composite metallocene polyethylene for packaging film can be used as a raw material for producing agricultural greenhouse film, packaging film and the like.

[0037] In the present invention, the above technical features can be freely combined to form a new technical solution without conflicting with each other.

[0038] Compared with the prior art, the technical solution of the present invention has the following beneficial technical effects: (1) Compared with the traditional physical blending method of multiple polyethylene materials and additives, the present invention mixes two different metallocene polyethylene base powders in a large spiral rotary feeder and then mixes them with the composite additives in a mixer. During the mixing process, the molecular chains of the two metallocene polyethylenes are rearranged under the stirring action of the screw, and the resulting composite metallocene polyethylene resin has excellent mechanical properties and processing properties; (2) The preparation method of the present invention does not require complicated adjustment of polymerization process parameters, and can quickly and effectively prepare metallocene polyethylene with both mechanical and processing properties, thereby greatly improving production efficiency; (3) The present invention can quickly and effectively improve the anti-aging performance of metallocene polyethylene in the field of pipe application by adding a composite additive (i.e., a combination of an antioxidant and a dispersant) in the post-system (i.e., an extrusion granulation system), thereby greatly reducing the difficulty of metallocene polyethylene development and production; (4) The production method of the present invention does not require large-scale transformation of existing raw material storage tanks, seed bins, catalyst filling systems, raw material feed control systems, and electrostatic control systems, thereby greatly reducing the cost of transformation investment; (5) The metallocene polyethylene produced by the preparation method of the present invention has the following properties: a melt mass flow rate of 0.5 g / 10 min to 3.5 g / 10 min, a density of 0.916 g / cm 3 Up to 0.935 g / cm 3 , tensile yield stress ≥18 MPa, dart impact strength ≥900 g, tensile fracture nominal strain ≥700%, critical shear rate>600 s -1 , yellow index ≤ 0; (6) When the metallocene polyethylene produced by the preparation method of the present invention replaces LLDPE and LDPE in the prior art in the production of polyethylene packaging film, the tensile yield stress increases by about 20%, the dart impact strength increases by about 75%, the tensile fracture strain increases by about 20%, and the critical shear rate is equivalent to that before. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be clearly and completely described below in combination with the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0040] Some embodiments of the present invention provide a composite metallocene polyethylene composition for packaging film, wherein the composite metallocene polyethylene composition comprises the following raw materials in parts by weight: 50 to 70 parts of the first metallocene polyethylene, 30 to 50 parts of the second metallocene polyethylene, 0.0002 to 0.002 parts of antioxidant, and 0.0002 to 0.002 parts of dispersant, wherein, The mechanical properties of the first metallocene polyethylene are better than those of the second metallocene polyethylene, and the processing properties of the second metallocene polyethylene are better than those of the first metallocene polyethylene.

[0041] In some embodiments, the first metallocene polyethylene is a polymer obtained by copolymerizing ethylene with 1-hexene or 1-butene in the presence of a first metallocene catalyst, and has a molecular weight distribution index of 2 to 3 (e.g., 2.2, 2.5 or 2.8) and a density of 0.916 g / cm 3 Up to 0.935 g / cm 3 (For example, 0.920 g / cm 3 , 0.925 g / cm 3 or 0.930 g / cm 3 ).

[0042] In some embodiments, the critical shear rate of the first metallocene polyethylene is 300 s -1 .

[0043] In some embodiments, the second metallocene polyethylene is a polymer obtained by copolymerizing ethylene with 1-hexene or 1-butene in the presence of a second metallocene catalyst, and has a molecular weight distribution width index of 3 to 4 (e.g., 3.2, 3.5 or 3.8) and a density of 0.916 g / cm 3 Up to 0.935 g / cm 3 (For example, 0.920 g / cm 3 , 0.925 g / cm 3 or 0.930 g / cm 3 ).

[0044] In some embodiments, the critical shear rate of the second metallocene polyethylene is 650 s -1 .

[0045] In some embodiments, the first metallocene polyethylene has a melt mass flow rate (MFR) of 0.5 g / l0 min to 3.5 g / l0 min (e.g., 1.0 g / l0 min, 1.5 g / l0 min, 2.0 g / l0 min, 2.5 g / l0 min, or 3.0 g / l0 min).

[0046] In some embodiments, the second metallocene polyethylene has a melt mass flow rate (MFR) of 0.5 g / l0 min to 3.5 g / l0 min (e.g., 1.0 g / l0 min, 1.5 g / l0 min, 2.0 g / l0 min, 2.5 g / l0 min, or 3.0 g / l0 min).

[0047] In some embodiments, the first metallocene catalyst and the second metallocene catalyst are different metallocene catalysts.

[0048] In some embodiments, the antioxidant includes at least one of antioxidant 1010, antioxidant 1076, and antioxidant 168, and the dispersant includes at least one of polyethylene wax and polyethylene glycol.

[0049] In the present invention, the first metallocene polyethylene has excellent mechanical properties but poor processing properties; the second metallocene polyethylene has excellent processing properties but poor mechanical properties. The present invention composites the first metallocene polyethylene and the second metallocene polyethylene together, striving to combine the excellent properties of the two into one, taking advantage of their strengths and avoiding their weaknesses, and obtaining a composite metallocene polyethylene material for packaging film that has both excellent processing properties and mechanical properties.

[0050] Some embodiments of the present invention also provide a method for preparing a composite metallocene polyethylene for packaging film, using any of the composite metallocene polyethylene compositions for packaging film as a raw material, and the preparation method comprises the following steps: 1) obtaining the first metallocene polyethylene and storing it for future use; 2) mixing the first metallocene polyethylene with the second metallocene polyethylene to obtain a metallocene polyethylene mixture; 3) Mixing the antioxidant and the dispersant to obtain a composite additive; 4) kneading the metallocene polyethylene mixture and the composite additive, and then cooling and pelletizing to obtain the composite metallocene polyethylene for packaging film.

[0051] In some embodiments, in the step 1), the first metallocene polyethylene is sealed with nitrogen during storage.

[0052] In the present invention, nitrogen is used to seal the first metallocene polyethylene to prevent the first metallocene polyethylene from being oxidized during storage.

[0053] In some embodiments, in step 2), the first metallocene polyethylene and the second metallocene polyethylene are mixed in a rotary feeder to obtain a metallocene polyethylene mixture.

[0054] In some embodiments, in step 2), the first metallocene polyethylene is mixed with the second metallocene polyethylene being produced in a rotary feeder (eg, a large screw rotary feeder).

[0055] In some embodiments, in the step 4), the mixing is performed using a mixer.

[0056] In some embodiments, in step 4), during the mixing process, the temperature of the extruder barrel is 250° C. to 280° C. (eg, 255° C., 260° C., 270° C., or 275° C.).

[0057] In the present invention, the two metallocene polyethylenes and the composite additives are added to a mixer for mixing. Under the action of high temperature, the two metallocene polyethylenes and related materials are melted, and then the two metallocene polyethylene molecular segments are disentangled and moved under the action of heat; under the stirring action of the screw, several molecular segments are rearranged. However, too high a temperature will cause the metallocene polyethylene material to degrade or cross-link, and too low a temperature will be unfavorable for processing the raw materials.

[0058] In some embodiments, in step 4), during the mixing process, the door opening is adjusted to 15% to 28% (eg, 16%, 18%, 20%, 22% or 25%).

[0059] In some embodiments, in step 4), the pelletizing water temperature used during pelletizing is less than 40° C. (eg, 20° C. or 30° C.).

[0060] In the present invention, after pelletizing water cooling and rotary pelletizing by a cutter, the mixed material of metallocene polyethylene extruded from a mixer is cooled in a very short time, wherein two metallocene polyethylene molecular chain segments are rearranged and then crystallized and solidified under the rapid cooling of pelletizing water, and finally a metallocene polyethylene having both mechanical properties and processing properties is obtained.

[0061] In the present invention, by controlling the parameters of the mixer, it is possible to ensure that the molecular segments of the two metallocene polyethylenes are rearranged during mixing, thereby achieving the purpose of taking into account both mechanical properties and processing properties. The preparation method of the present invention takes into account both the processing properties and mechanical properties of the metallocene polyethylene product, has a simple process, low cost, and does not require the introduction of other special raw materials.

[0062] Some embodiments of the present invention also provide a composite metallocene polyethylene for packaging film prepared by any of the above-mentioned preparation methods.

[0063] In some embodiments, the composite metallocene polyethylene for packaging film has the following characteristics: Melt mass flow rate is 0.5 g / 10 min to 3.5 g / 10 min, density is 0.916 g / cm 3 Up to 0.935g / cm 3 , tensile yield stress ≥18 MPa, dart impact strength ≥900 g, tensile fracture nominal strain ≥700%, critical shear rate>600 s -1 , yellow index ≤0.

[0064] In this field, the standards for metallocene polyethylene with excellent mechanical properties are: tensile yield stress ≥18 MPa, dart impact strength ≥900 g, tensile fracture nominal strain ≥700%; the standards for metallocene polyethylene with excellent processing properties are: critical shear rate >600 s -1 In addition, the yellowness index of the raw materials must be ≤0.

[0065] Therefore, the composite metallocene polyethylene for packaging film provided by the present invention has both excellent mechanical properties and processing properties.

[0066] In some embodiments, the composite metallocene polyethylene for packaging film can be used as a raw material for producing agricultural greenhouse films, packaging films, and the like.

[0067] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0068] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.

[0069] In the present invention, the melt mass flow rate (or melt index) of the composite metallocene polyethylene is tested according to the national standard GB / T3682, the density is tested according to the national standard GB / T 1033.2, the tensile yield stress and tensile fracture nominal strain are tested according to the national standard GB / T 1040.2, and the dart impact strength is tested according to the national standard GB / T 9639.1. The critical shear rate detection conditions are as follows: temperature is 190°C, capillary aspect ratio is 30:1, and the shear rate range is 1 s -1 ~1000 s -1 .

[0070] Example 1 A method for preparing composite metallocene polyethylene for packaging film comprises the following steps: S1: Obtain the first metallocene polyethylene (molecular weight distribution 2 to 3, critical shear rate 300s -1 ), store for future use; S2: 50 parts by weight of a first metallocene polyethylene (molecular weight distribution 2 to 3, critical shear rate 300 s -1 ) and 50 parts by weight of a second metallocene polyethylene (molecular weight distribution 3 to 4, critical shear rate 650s -1) are fed separately, fully mixed in a large spiral rotating feeder, and the two metallocene polyethylenes are mixed evenly by physical mixing means to obtain a metallocene polyethylene mixture; S3: 0.002 parts by weight of antioxidant 1076 and 0.002 parts by weight of dispersant polyethylene wax are mixed uniformly to obtain a composite additive; S4: adding the metallocene polyethylene mixture and the composite additive into a mixer for mixing, then cooling and pelletizing to obtain composite metallocene polyethylene for packaging film, i.e., metallocene polyethylene resin; wherein, the extruder barrel temperature is 255°C, the door opening is adjusted to 25%, and the pelletizing water temperature is 38°C.

[0071] The packaging film prepared in this embodiment is used to prepare a polyethylene packaging film using the composite metallocene polyethylene.

[0072] The properties of the metallocene polyethylene resin and polyethylene packaging film prepared in this example were tested. The results showed that the melt index was 1 g / 10 min and the density was 0.920 g / cm 3 , tensile yield stress is 20 MPa, dart impact strength is 1100 g, tensile fracture nominal strain is 850%, critical shear rate is 650 s -1 In addition, the yellowness index of the metallocene polyethylene resin is -2.3.

[0073] Therefore, the composite metallocene polyethylene and polyethylene packaging film prepared in this embodiment not only meets the standards of metallocene polyethylene with excellent mechanical properties, but also meets the standards of metallocene polyethylene with excellent processing properties, and has both excellent mechanical properties and processing properties.

[0074] Example 2 A method for preparing composite metallocene polyethylene for packaging film comprises the following steps: S1: Obtain the first metallocene polyethylene (molecular weight distribution 2 to 3, critical shear rate 300s -1 ), store for future use; S2: 70 parts by weight of a first metallocene polyethylene (molecular weight distribution 2 to 3, critical shear rate 300 s -1 ) and 30 parts by weight of a second metallocene polyethylene (molecular weight distribution 3 to 4, critical shear rate 650s -1 ) are fed separately, fully mixed in a large spiral rotating feeder, and the two metallocene polyethylenes are mixed evenly by physical mixing means to obtain a metallocene polyethylene mixture; S3: 0.002 parts by weight of antioxidant 1076 and 0.002 parts by weight of dispersant polyethylene wax are mixed uniformly to obtain a composite additive; S4: adding the metallocene polyethylene mixture and the composite additive into a mixer for mixing, then cooling and pelletizing to obtain composite metallocene polyethylene for packaging film, i.e., metallocene polyethylene resin; wherein, the extruder barrel temperature is 255° C., the door opening is adjusted to 20%, and the pelletizing water temperature is 38° C.

[0075] The composite metallocene polyethylene prepared in this example is used to prepare a polyethylene packaging film.

[0076] The properties of the metallocene polyethylene resin and polyethylene packaging film prepared in this example were tested. The results showed that the melt index was 1 g / 10 min and the density was 0.920 g / cm 3 , tensile yield stress is 25 MPa, dart impact strength is 1350 g, tensile fracture nominal strain is 900%, and critical shear rate is 635 s -1 .

[0077] Therefore, the composite metallocene polyethylene and polyethylene packaging film prepared in this embodiment not only meets the standards of metallocene polyethylene with excellent mechanical properties, but also meets the standards of metallocene polyethylene with excellent processing properties, and has both excellent mechanical properties and processing properties.

[0078] Comparative Example 1 A method for preparing composite metallocene polyethylene for packaging film comprises the following steps: S1: 40 parts by weight of a first metallocene polyethylene (molecular weight distribution 2 to 3, critical shear rate 300 s -1 ) and 60 parts by weight of a second metallocene polyethylene (molecular weight distribution 3 to 4, critical shear rate 650 s -1 ) are fed separately, fully mixed in a large spiral rotating feeder, and the two metallocene polyethylenes are mixed evenly by physical mixing means to obtain a metallocene polyethylene mixture; S2: 0.002 parts by weight of antioxidant 1076 and 0.002 parts by weight of dispersant polyethylene wax are mixed uniformly to obtain a composite additive; S3: adding the metallocene polyethylene mixture and the composite additive into a mixer for mixing, and then cooling and pelletizing to obtain composite metallocene polyethylene, i.e., metallocene polyethylene resin; wherein, the extruder barrel temperature is 255°C, the door opening is adjusted to 25%, and the pelletizing water temperature is 38°C.

[0079] S4: preparing a polyethylene packaging film using the composite metallocene polyethylene prepared in step S3.

[0080] The properties of the metallocene polyethylene resin and packaging film prepared in this comparative example were tested. The results showed that the melt index was 1 g / 10 min and the density was 0.920 g / cm 3, tensile yield stress is 16.5 MPa, dart impact strength is 720 g, tensile fracture nominal strain is 900%, critical shear rate is 500 s -1 ; It cannot meet the excellent mechanical properties standards of polyethylene packaging film (tensile yield stress ≥18 MPa, dart impact strength ≥900 g, tensile fracture nominal strain ≥700%); nor can it meet the standards of excellent processing performance (critical shear rate >600 s -1 ).

[0081] Comparative Example 2 A method for preparing composite metallocene polyethylene for packaging film comprises the following steps: S1: 70 parts by weight of a first metallocene polyethylene (molecular weight distribution 2 to 3, critical shear rate 300 s -1 ) and 30 parts by weight of a second metallocene polyethylene (molecular weight distribution 3 to 4, critical shear rate 650 s -1 ) are fed separately, fully mixed in a large spiral rotating feeder, and the two metallocene polyethylenes are mixed evenly by physical mixing means to obtain a metallocene polyethylene mixture; S2: 0.002 parts by weight of antioxidant 1076 and 0.002 parts by weight of dispersant polyethylene wax are mixed uniformly to obtain a composite additive; S3: adding the metallocene polyethylene mixture and the composite additive into a mixer for mixing, then cooling and pelletizing to obtain composite metallocene polyethylene for packaging film, i.e., metallocene polyethylene resin; wherein the extruder barrel temperature is 255° C., the door opening is adjusted to 10%, and the pelletizing water temperature is 38° C.

[0082] S4: preparing a polyethylene packaging film from the composite metallocene polyethylene prepared in step S3.

[0083] The properties of the metallocene polyethylene resin and packaging film prepared in this comparative example were tested. The results showed that the melt index was 1 g / 10 min and the density was 0.920 g / cm 3 , tensile yield stress is 25 MPa, dart impact strength is 950 g, tensile fracture nominal strain is 900%, critical shear rate is 435 s -1 ; It cannot meet the standard of excellent mechanical properties of metallocene polyethylene (tensile yield stress ≥18 MPa, dart impact strength ≥900 g, tensile fracture nominal strain ≥700%); it also cannot meet the standard of excellent processing performance (critical shear rate >600 s -1 ).

[0084] Comparative Example 3 A method for preparing a conventional polyethylene film comprises the following steps: S1: 30 parts by weight of a first metallocene polyethylene (molecular weight distribution 2 to 3, critical shear rate 300 s -1 ), 20 parts by weight of LDPE (molecular weight distribution 3 to 4, critical shear rate 950 s -1 ), 50 parts by weight of LLDPE (molecular weight distribution 3 to 4, critical shear rate 350 s -1 ) for physical mixing; S2: Prepare polyethylene packaging film using the composite metallocene polyethylene prepared in this comparative example.

[0085] The properties of the metallocene polyethylene resin and packaging film prepared in this comparative example were tested. The results showed that the melt index was 1.4 g / 10 min and the density was 0.922 g / cm 3 , tensile yield stress is 15.5 MPa, dart impact strength is 120 g, tensile fracture nominal strain is 640%, and critical shear rate is 600 s -1 Although it meets the standard of excellent processing performance, it cannot meet the standard of excellent mechanical properties of metallocene polyethylene (tensile yield stress ≥18 MPa, dart impact strength ≥900 g, tensile fracture nominal strain ≥700%), and thus has a significant gap in mechanical properties compared with the polyethylene film for packaging prepared using composite metallocene polyethylene in Examples 1 and 2.

[0086] Comparative Example 4 A method for preparing a conventional polyethylene film comprises the following steps: S1: 50 parts by weight of a second metallocene polyethylene (molecular weight distribution 3 to 4, critical shear rate 650 s -1 ), 20 parts by weight of LDPE (molecular weight distribution 3 to 4, critical shear rate 950 s -1 ), 30 parts by weight of LLDPE (molecular weight distribution 3 to 4, critical shear rate 350 s -1 ) are physically mixed to obtain a composite metallocene polyethylene; S2: preparing a polyethylene packaging film using the composite metallocene polyethylene obtained in step S1.

[0087] The properties of the composite metallocene polyethylene and packaging film prepared in this comparative example were tested, and the results showed that the melt index was 1.2 g / 10 min and the density was 0.921 g / cm 3 , tensile yield stress is 16.0 MPa, dart impact strength is 100 g, tensile fracture nominal strain is 620%, critical shear rate is 620 s -1Although it meets the standard of having excellent processing performance, it cannot meet the standard of excellent mechanical properties of metallocene polyethylene (tensile yield stress ≥18 MPa, dart impact strength ≥900 g, tensile fracture nominal strain ≥700%), and thus has a significant performance gap with the mechanical properties of the polyethylene film for packaging prepared using the composite metallocene polyethylene in Examples 1 and 2.

[0088] Comparative Example 5 A method for preparing composite metallocene polyethylene for packaging film comprises the following steps: S1: 50 parts by weight of a first metallocene polyethylene (molecular weight distribution 2 to 3, critical shear rate 300 s -1 ) and 50 parts by weight of a second metallocene polyethylene (molecular weight distribution 3 to 4, critical shear rate 650 s -1 ) are fed separately, fully mixed in a large spiral rotating feeder, and the two metallocene polyethylenes are mixed evenly by physical mixing means to obtain a metallocene polyethylene mixture; S2: 0.01 parts by weight of antioxidant 1076 and 0.002 parts by weight of dispersant polyethylene wax are mixed uniformly to obtain a composite additive; S3: adding the metallocene polyethylene mixture and the composite additive into a mixer for mixing, and then cooling and pelletizing to obtain composite metallocene polyethylene for packaging film; wherein, the extruder barrel temperature is 255°C, the door opening is adjusted to 25%, and the pelletizing water temperature is 38°C.

[0089] S4: using the composite metallocene polyethylene prepared in this example to prepare a polyethylene packaging film.

[0090] The performance of the metallocene polyethylene resin prepared in this comparative example was tested, and the results showed that the yellow index was 3.1, which did not meet the requirement of yellow index of metallocene polyethylene resin ≤ 0. It can be seen that the high content of antioxidants in the composite metallocene polyethylene composition easily causes the yellow index of the composite metallocene polyethylene for packaging film to fail to meet the requirements.

[0091] In summary, compared with the polyethylene packaging film prepared by the conventional method, the molecular chain segments of the composite metallocene polyethylene for packaging film according to the present invention have metallocene polyethylene with a molecular weight distribution of 2 to 3 with poor processing performance and excellent mechanical properties, and metallocene polyethylene with a molecular weight distribution of 3 to 4 with poor mechanical properties and excellent processing performance. Under the action of a mixer, the molecular chain segments of the two metallocene polyethylenes are rearranged, crystallized and solidified, thereby forming a metallocene polyethylene with both processing performance and mechanical properties.

[0092] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0093] In the present application, in the absence of any contrary description, the directional words used, such as "upper" and "lower", are specifically the directions of the drawings. In addition, in the description of the present specification, the terms "including", "comprising", etc. refer to "including but not limited to". In this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of the associated objects, indicating that there may be three relationships, for example, A and / or B, which can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A, B can be singular or plural. In this article, "at least one" refers to one or more, and "multiple" refers to two or more. "At least one", "at least one of the following (individuals)" or similar expressions thereof refer to any combination of these items, including any combination of singular (individuals) or plural (individuals). For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc, or abc, where a, b, c can be single or plural, respectively.

[0094] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A composite metallocene polyethylene composition for packaging film, characterized in that: The following raw materials are included in parts by weight: 50 to 70 parts of a first metallocene polyethylene, 30 to 50 parts of a second metallocene polyethylene, 0.0002 to 0.002 parts of an antioxidant, and 0.0002 to 0.002 parts of a dispersant, wherein the first metallocene polyethylene is a polymer obtained by copolymerizing ethylene with 1-hexene or 1-butene in the presence of a first metallocene catalyst, and the molecular weight distribution index is 2 to 3, and the second metallocene polyethylene is a polymer obtained by copolymerizing ethylene with 1-hexene or 1-butene in the presence of a second metallocene catalyst, and the molecular weight distribution index is 3 to 4.

2. The composite metallocene polyethylene composition for packaging film according to claim 1, characterized in that: The critical shear rate of the first metallocene polyethylene is 300 s -1 ; The critical shear rate of the second metallocene polyethylene is 650 s -1 .

3. The composite metallocene polyethylene composition for packaging film according to claim 1 or 2, characterized in that: The density of the first metallocene polyethylene is 0.916 g / cm 3 Up to 0.935 g / cm 3 ; The density of the second metallocene polyethylene is 0.916 g / cm 3 Up to 0.935 g / cm 3 .

4. The composite metallocene polyethylene composition for packaging film according to claim 3, characterized in that: The melt mass flow rate of the first metallocene polyethylene is 0.5 g / l0 min to 3.5 g / l0 min; The melt mass flow rate of the second metallocene polyethylene is 0.5 g / l0 min to 3.5 g / l0 min.

5. The composite metallocene polyethylene composition for packaging film according to claim 1, 2 or 4, characterized in that: The antioxidant includes at least one of antioxidant 1076, antioxidant 1010 and antioxidant 168; The dispersant includes at least one of polyethylene wax and polyethylene glycol.

6. A method for preparing composite metallocene polyethylene for packaging film, characterized in that: Using the composite metallocene polyethylene composition for packaging film according to any one of claims 1 to 5 as a raw material, the preparation method comprises the following steps: 1) obtaining the first metallocene polyethylene and storing it for future use; 2) mixing the first metallocene polyethylene with the second metallocene polyethylene to obtain a metallocene polyethylene mixture; 3) Mixing the antioxidant and the dispersant to obtain a composite additive; 4) kneading the metallocene polyethylene mixture and the composite additive, and then cooling and pelletizing to obtain the composite metallocene polyethylene for packaging film.

7. The method for preparing composite metallocene polyethylene for packaging film according to claim 6, characterized in that: In the step 1), the first metallocene polyethylene is sealed with nitrogen during storage.

8. The method for preparing composite metallocene polyethylene for packaging film according to claim 7, characterized in that: In the step 2), the first metallocene polyethylene and the second metallocene polyethylene are mixed in a rotary feeder.

9. The method for preparing composite metallocene polyethylene for packaging film according to claim 7 or 8, characterized in that: In the step 2), the first metallocene polyethylene is mixed with the second metallocene polyethylene being produced in a rotary feeder.

10. The method for preparing composite metallocene polyethylene for packaging film according to claim 9, characterized in that: In the step 4), the mixing is performed using a mixer.

11. The method for preparing composite metallocene polyethylene for packaging film according to claim 7, 8 or 10, characterized in that: In the step 4), during the mixing process, the temperature of the extruder barrel is 250° C. to 280° C., and the door opening is adjusted to 15% to 28%.

12. The method for preparing composite metallocene polyethylene for packaging film according to claim 11, characterized in that: In the step 4), the temperature of pelletizing water used during pelletizing is less than 40°C.

13. A composite metallocene polyethylene for packaging film, characterized in that: The composite metallocene polyethylene for packaging film is prepared by the preparation method according to any one of claims 6 to 12.

Citation Information

Patent Citations

  • Metallocene polyethylene greenhouse film resin composition

    CN102167855A

  • Highly-transparent polyethylene composition and preparation method thereof

    CN103772797A

  • Thinning type FFS (fringe field switching) film for heavy packaging and preparation method thereof

    CN114454579A

  • Preparation method of polyethylene, polyethylene and polyethylene composition

    CN115677894A

  • Process for preparing linear low density polyethylene

    KR1020070098276A