High-strength and high-toughness PP material and preparation method thereof

By adding fillers such as calcium carbonate, silica, tin powder to the polypropylene material, and using modifiers such as pentaerythritol tetraacrylate and maleic anhydride grafted polypropylene, the toughness and stretching of traditional polypropylene materials are solved. The problem of insufficient strength has achieved high strength and high toughness PP material preparation, improving the impact resistance of the material.

CN118994785AInactive Publication Date: 2024-11-22广东精一塑胶实业有限公司
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411279143.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional polypropylene materials have shortcomings in tensile strength and toughness, especially when facing external forces such as impact and vibration, which can easily lead to brittle fracture, reducing the reliability and service life of the product.

Method used

The toughness of the material is enhanced by adding calcium carbonate, silica and tin powder, and grafting polypropylene with pentaerythritol tetraacrylate and maleic anhydride to improve the compatibility of fillers and polypropylene, and in combination with methyl silicone oil promotes crystallization in the amorphous region. , forming PP materials with high tensile strength and toughness.

Benefits of technology

It significantly improves the toughness and tensile strength of PP materials, enhances the impact resistance and reliability of the materials, and meets the application needs of high strength and high toughness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005041109250000041
    Figure BDA0005041109250000041
  • Figure BDA0005041109250000051
    Figure BDA0005041109250000051
  • Figure BDA0005041109250000052
    Figure BDA0005041109250000052
Patent Text Reader

Abstract

The invention relates to a high-strength and high-toughness PP material and a preparation method, and belongs to the technical field of PP materials, and the PP material comprises the following raw materials: polypropylene, pentaerythritol tetraacrylate, maleic anhydride grafted polypropylene, calcium carbonate, silicon dioxide, tin powder and methyl silicone oil. The calcium carbonate, the silicon dioxide and the tin powder are added and start from three different dimensions of absorbing impact energy, blocking or terminating cracks and inducing beta crystal form formation respectively, so that the toughness of a PP material finished product is synergistically improved; on the basis, pentaerythritol tetraacrylate is used for providing more nucleation sites for the system, maleic anhydride grafted polypropylene is added to play a role in forming calcium salt with calcium carbonate and a certain interface transformation role, the compatibility of system filler and polypropylene is further improved, and then the toughness of a PP material finished product is reinforced in an auxiliary mode. In addition, the added methyl silicone oil promotes crystallization of an amorphous region of polypropylene, and the tensile strength of a PP material finished product is improved to a certain extent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of PP materials, and in particular, relates to a high-strength and high-toughness PP material and a preparation method thereof. Background Art

[0002] As an important polymer material, polypropylene (PP) is widely used in many fields such as home furniture, automobiles, home appliances, packaging, and construction due to its advantages such as low price, good processing performance, and strong chemical stability. For example, in the field of home furniture, polypropylene is often used in storage cabinets, chairs, containers and other products; in the field of automobile manufacturing, polypropylene is often used in automotive interior parts, bumpers and other parts; in the electronic and electrical industry, polypropylene can be used to manufacture electrical housings, wires and cables, etc.; in terms of packaging materials, polypropylene is widely used to make various containers and films. Today, polypropylene has become one of the fastest-growing plastic varieties, and its output is second only to polyethylene and polyvinyl chloride.

[0003] However, traditional polypropylene materials have certain limitations in performance. On the one hand, its tensile strength often cannot meet the requirements of certain special engineering structures or application scenarios with high material strength requirements; on the other hand, when faced with external forces such as impact and vibration, the low toughness of ordinary polypropylene materials can easily lead to brittle fracture of the material, reducing the reliability and service life of the product. Therefore, in order to overcome these problems, it is of great practical significance and broad application prospects to develop a PP material with high tensile strength and toughness to meet the ever-evolving market demand and increasingly stringent application requirements through methods such as modification of polypropylene and addition of specific fillers. Summary of the invention

[0004] The purpose of the present invention is to provide a high-strength and high-toughness PP material and a preparation method. The present invention adds calcium carbonate, silicon dioxide and tin powder, respectively starting from three different dimensions of absorbing impact energy, hindering or terminating cracks, and inducing the formation of β crystals, to synergistically increase the toughness of the finished PP material; on this basis, the present invention also uses pentaerythritol tetraacrylate as the system to provide more nucleation sites, and adds maleic anhydride grafted polypropylene to play a role in forming calcium salts and certain interface transformation with calcium carbonate, further improving the compatibility of the system filler and polypropylene, thereby assisting in strengthening the toughness of the finished PP material. In addition, the methyl silicone oil added in the present invention promotes the crystallization of the non-crystalline region of polypropylene, increases the tensile strength of the finished PP material to a certain extent, and solves the problem of the lack of toughness and tensile strength of the PP material in the prior art.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A high-strength and high-toughness PP material, the PP material comprises the following raw materials:

[0007] Polypropylene, pentaerythritol tetraacrylate, maleic anhydride grafted polypropylene, calcium carbonate, silica, tin powder and methyl silicone oil.

[0008] As a preferred technical solution of the present invention, the polypropylene is 100-110 parts by weight, the pentaerythritol tetraacrylate is 1.5-2 parts by weight, the maleic anhydride grafted polypropylene is 8-10 parts by weight, the calcium carbonate is 6-8 parts by weight, the silicon dioxide is 4-5 parts by weight, the tin powder is 5-6 parts by weight, and the methyl silicone oil is 3-5 parts by weight.

[0009] As a preferred technical solution of the present invention, the grafting rate of the maleic anhydride grafted polypropylene is 1.0%.

[0010] As a preferred technical solution of the present invention, the particle size of the calcium carbonate is 70-80nm.

[0011] As a preferred technical solution of the present invention, the silica particle size is 50-60nm.

[0012] A method for preparing a high-strength and high-toughness PP material, the preparation method specifically comprising the following steps:

[0013] S1. Raw material pretreatment: drying polypropylene, pentaerythritol tetraacrylate and silicon dioxide under controlled temperature, and drying maleic anhydride grafted polypropylene and calcium carbonate under controlled temperature and vacuum;

[0014] S2. Put the dried polypropylene, dried pentaerythritol tetraacrylate, methyl silicone oil, dried maleic anhydride grafted polypropylene, dried calcium carbonate, dried silicon dioxide and tin powder into the extruder in sequence, set the temperature and speed of mixing, extrusion and die head, melt-extrude and granulate to obtain the finished PP material.

[0015] As a preferred technical solution of the present invention, the temperature of the temperature-controlled drying in step S1 is 80-85° C. and the time is 8-10 hours.

[0016] As a preferred technical solution of the present invention, the temperature of the temperature-controlled vacuum drying in step S1 is 95-100° C. and the time is 6-8 hours.

[0017] As a preferred technical solution of the present invention, the mixing temperature in step S2 is 175-180°C, the extrusion temperature is 190-195°C, and the die temperature is 180-185°C.

[0018] As a preferred technical solution of the present invention, the rotation speeds of the mixing, extrusion and die head in step S2 are all 40-50 r / min.

[0019] Beneficial effects of the present invention:

[0020] (1) The present invention selects calcium carbonate and silicon dioxide with insufficient coordination and high specific surface area, and uses their own large number of unsaturated residual bonds to form bonds with groups in polypropylene, so that they have the characteristic of being easily distributed in the bond gaps of polypropylene, reducing the disadvantage of incompatibility between fillers and polypropylene; in addition, the calcium carbonate added in the present invention can effectively absorb impact energy when the PP material product is impacted, and the added silicon dioxide can effectively hinder the crack propagation or passivate and terminate the crack, thereby increasing the toughness of the material; on this basis, the present invention also adds tin powder with a high specific surface area to act as a heterogeneous nucleating agent, inducing polypropylene to form a β crystal, thereby improving the toughness of the PP material product; that is, the calcium carbonate, silicon dioxide and tin powder added in the present invention can respectively absorb impact energy, hinder or terminate cracks, and induce the formation of β crystals from three different dimensions, thereby synergistically increasing the toughness of the PP material product;

[0021] On this basis, the present invention further adds pentaerythritol tetraacrylate modified polypropylene to provide more nucleation sites for the system, and adds maleic anhydride grafted polypropylene. Maleic anhydride grafted polypropylene can form calcium salt with calcium carbonate, and to a certain extent can act as a nucleating agent and work together with tin powder to increase the induction of polypropylene to form β crystal form; in addition, maleic anhydride grafted polypropylene also has a certain interface transformation effect, which can transform the polypropylene-filler interface in the system into two interfaces of polypropylene-maleic anhydride grafted polypropylene and maleic anhydride grafted polypropylene-filler. Due to the transformation of the interface in the system, the compatibility of the filler and polypropylene in the system is further improved, thereby assisting in strengthening the toughness of the PP material product.

[0022] (2) The addition of methyl silicone oil in the present invention promotes the crystallization of the non-crystalline region of polypropylene, thereby making the crystalline region of polypropylene larger and increasing its density. The molecular chains in the system are arranged more closely and orderly, thereby increasing the tensile strength of the finished PP material to a certain extent. DETAILED DESCRIPTION

[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Example 1

[0025] A high-strength and high-toughness PP material, the PP material comprises the following raw materials in parts by weight:

[0026]

[0027] The grafting rate of the maleic anhydride grafted polypropylene is 1.0%;

[0028] A method for preparing a high-strength and high-toughness PP material, the preparation method specifically comprising the following steps:

[0029] S1. Raw material pretreatment: polypropylene, pentaerythritol tetraacrylate and silicon dioxide were dried at 80°C for 10 hours, and maleic anhydride grafted polypropylene and calcium carbonate were vacuum dried at 100°C for 6 hours;

[0030] S2. Put the dried polypropylene, dried pentaerythritol tetraacrylate, methyl silicone oil, dried maleic anhydride grafted polypropylene, dried calcium carbonate, dried silicon dioxide and tin powder into the extruder in sequence, set the mixing temperature to 178°C, the extrusion temperature to 195°C, the die temperature to 180°C, the rotation speed to 50r / min, melt-extrude and granulate to obtain the finished PP material.

[0031] Example 2

[0032] A high-strength and high-toughness PP material, the PP material comprises the following raw materials in parts by weight:

[0033]

[0034] The grafting rate of the maleic anhydride grafted polypropylene is 1.0%;

[0035] A method for preparing a high-strength and high-toughness PP material, the preparation method specifically comprising the following steps:

[0036] S1. Raw material pretreatment: polypropylene, pentaerythritol tetraacrylate and silicon dioxide were dried at 85°C for 8 hours, and maleic anhydride grafted polypropylene and calcium carbonate were vacuum dried at 95°C for 7 hours;

[0037] S2. Put the dried polypropylene, dried pentaerythritol tetraacrylate, methyl silicone oil, dried maleic anhydride grafted polypropylene, dried calcium carbonate, dried silicon dioxide and tin powder into the extruder in sequence, set the mixing temperature to 180°C, the extrusion temperature to 190°C, the die temperature to 183°C, the rotation speed to 40r / min, melt-extrude and granulate to obtain the finished PP material.

[0038] Example 3

[0039] A high-strength and high-toughness PP material, the PP material comprises the following raw materials in parts by weight:

[0040]

[0041] The grafting rate of the maleic anhydride grafted polypropylene is 1.0%;

[0042] A method for preparing a high-strength and high-toughness PP material, the preparation method specifically comprising the following steps:

[0043] S1. Raw material pretreatment: polypropylene, pentaerythritol tetraacrylate and silicon dioxide were dried at 83°C for 9 hours, and maleic anhydride grafted polypropylene and calcium carbonate were vacuum dried at 98°C for 8 hours;

[0044] S2. Put the dried polypropylene, dried pentaerythritol tetraacrylate, methyl silicone oil, dried maleic anhydride grafted polypropylene, dried calcium carbonate, dried silicon dioxide and tin powder into the extruder in sequence, set the mixing temperature to 175°C, the extrusion temperature to 193°C, the die temperature to 185°C, the rotation speed to 45r / min, melt-extrude and granulate to obtain the finished PP material.

[0045] Comparative Example 1

[0046] Compared with Example 3, the difference is that in Comparative Example 1, no calcium carbonate is added, but the silicon dioxide is 7.5 parts by weight, the tin powder is 9.5 parts by weight, and the other operating steps and parameters remain unchanged.

[0047] Comparative Example 2

[0048] Compared with Example 3, the difference is that in Comparative Example 2, no silicon dioxide is added, while calcium carbonate is 9 parts by weight and tin powder is 8 parts by weight, and the other operating steps and parameters remain unchanged.

[0049] Comparative Example 3

[0050] Compared with Example 3, the difference is that in Example 3, no tin powder is added, but calcium carbonate is 10 parts by weight, silicon dioxide is 7 parts by weight, and the other operating steps and parameters remain unchanged.

[0051] Comparative Example 4

[0052] Compared with Example 3, the difference is that pentaerythritol tetraacrylate is not added in Comparative Example 4, and the other operating steps and parameters remain unchanged.

[0053] Comparative Example 5

[0054] Compared with Example 3, the difference is that in Comparative Example 5, maleic anhydride grafted polypropylene is not added, and the other operating steps and parameters remain unchanged.

[0055] Comparative Example 6

[0056] Compared with Example 3, the difference is that no methyl silicone oil is added in Comparative Example 6, and the other operating steps and parameters remain unchanged.

[0057] Test Example 1

[0058] Toughness test: According to GB / T 1043.1-2008, the test temperature is 23° C. The notched impact strength test was performed on the PP material products prepared in Examples 1-3 and Comparative Examples 1-5; the results are shown in Table 1.

[0059] Table 1

[0060] <![CDATA[Notched impact strength (kJ·m -2 )]]> Example 1 45.3 Example 2 45.0 Example 3 45.7 Comparative Example 1 38.5 Comparative Example 2 37.4 Comparative Example 3 35.9 Comparative Example 4 32.6 Comparative Example 5 30.1

[0061] As can be seen from Table 1, the PP material product prepared by the present invention has excellent toughness. This is because the calcium carbonate, silicon dioxide and tin powder added in the present invention can respectively absorb impact energy, hinder or terminate cracks, and induce the formation of β crystals in three different dimensions, and synergistically increase the toughness of the PP material product; on this basis, the present invention also adds pentaerythritol tetraacrylate to provide more nucleation sites for the system, and adds maleic anhydride grafted polypropylene, which can form calcium salt with calcium carbonate. In addition, maleic anhydride grafted polypropylene also has a certain interface transformation effect, which can further improve the compatibility of fillers and polypropylene in the system and thus assist in strengthening the toughness of the PP material product.

[0062] Test Example 2

[0063] Tensile strength test: According to GB / T1040-20, the tensile strength test was performed on the PP material finished products prepared in Examples 1-3 and Comparative Example 6; the results are shown in Table 2.

[0064] Table 2

[0065] Tensile strength(MPa) Example 1 75.9 Example 2 75.5 Example 3 76.4 Comparative Example 1 47.8

[0066] It can be seen from Table 2 that the PP material product prepared by the present invention has outstanding tensile strength. Specifically, the methyl silicone oil added in the present invention promotes the crystallization of the non-crystalline region of polypropylene, thereby making the crystalline region of polypropylene larger and the density increased, and the molecular chains in the system are arranged more closely and orderly, thereby increasing the tensile strength of the PP material product to a certain extent.

[0067] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0068] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A high-strength and high-toughness PP material, characterized in that: The PP material includes the following raw materials: Polypropylene, pentaerythritol tetraacrylate, maleic anhydride grafted polypropylene, calcium carbonate, silica, tin powder and methyl silicone oil.

2. The high-strength and high-toughness PP material according to claim 1, characterized in that: The polypropylene is 100-110 parts by weight, the pentaerythritol tetraacrylate is 1.5-2 parts by weight, the maleic anhydride grafted polypropylene is 8-10 parts by weight, the calcium carbonate is 6-8 parts by weight, the silicon dioxide is 4-5 parts by weight, the tin powder is 5-6 parts by weight, and the methyl silicone oil is 3-5 parts by weight.

3. The high-strength and high-toughness PP material according to claim 1, characterized in that: The grafting rate of the maleic anhydride grafted polypropylene is 1.0%.

4. The high-strength and high-toughness PP material according to claim 1, characterized in that: The calcium carbonate particle size is 70-80 nm.

5. The high-strength and high-toughness PP material according to claim 1, characterized in that: The silica particle size is 50-60 nm.

6. A method for preparing the high-strength and high-toughness PP material according to any one of claims 1 to 5, characterized in that: The preparation method specifically comprises the following steps: S1. Raw material pretreatment: drying polypropylene, pentaerythritol tetraacrylate and silicon dioxide under controlled temperature, and drying maleic anhydride grafted polypropylene and calcium carbonate under controlled temperature and vacuum; S2. Put the dried polypropylene, dried pentaerythritol tetraacrylate, methyl silicone oil, dried maleic anhydride grafted polypropylene, dried calcium carbonate, dried silicon dioxide and tin powder into the extruder in sequence, set the temperature and speed of mixing, extrusion and die head, melt-extrude and granulate to obtain the finished PP material.

7. The method for preparing the high-strength and high-toughness PP material according to claim 5, characterized in that: The temperature of the temperature-controlled drying in step S1 is 80-85° C. and the time is 8-10 hours.

8. The method for preparing the high-strength and high-toughness PP material according to claim 5, characterized in that: The temperature of the temperature-controlled vacuum drying in step S1 is 95-100° C. and the time is 6-8 hours.

9. The method for preparing the high-strength and high-toughness PP material according to claim 5, characterized in that: In step S2, the mixing temperature is 175-180°C, the extrusion temperature is 190-195°C, and the die temperature is 180-185°C.

10. The method for preparing the high-strength and high-toughness PP material according to claim 5, characterized in that: The rotation speeds of the mixing, extrusion and die head in step S2 are all 40-50 r / min.

Citation Information

Patent Citations

  • High-rigidity and high-toughness polypropylene composite material and preparation method thereof

    CN109575450A

  • Polypropylene toughening master batch as well as preparation method and application thereof

    CN117164989A

  • High-toughness easy-to-demould polypropylene material and preparation method thereof

    CN117186548A

  • Plant fiber / pp composite material and preparation method thereof

    CN117603584A