Preparation method of stretchable flexible heat conduction material

By adding boron nitride (BN) to the P(M-PDA-EGDMA) polymer substrate and preparing porous fiber structures using 3D printing technology, the thermal conductivity of traditional thermal conductivity materials in flexible electronic equipment and high temperature environments is solved. and performance decay problem, achieving a combination of high thermal conductivity and flexibility, suitable for modern electronic equipment and high temperature management systems.

CN118994831AActive Publication Date: 2024-11-22TIANJIN UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411210638.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-22
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

Traditional thermally conductive materials show uneven thermal conductivity and decay in flexible electronic equipment and high temperature environments, making it difficult to meet the needs of modern electronic equipment for high thermal conductivity and flexible materials.

Method used

P(M-PDA-EGDMA) is used as the polymer substrate, combined with boron nitride (BN) as a high thermal conductivity filler, and a three-dimensional porous fiber structure is prepared through 3D printing technology to fill boron nitride nanoparticles to form stretchable flexible thermal conductivity Material.

Benefits of technology

It achieves high thermal conductivity and excellent flexibility in high temperature environments, extends the service life of the material, and is suitable for modern electronic equipment and high temperature management systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994831A_ABST
    Figure CN118994831A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a stretchable flexible heat conduction material, which comprises the following steps: synthesis of P (M-PDA-EGDMA): placing EGDMA, M-PDA and an initiator in a container of N, N-dimethylformamide DMF, introducing argon into the mixture, heating the mixture to 55-65 DEG C, stirring and polymerizing to obtain a reaction mixture; preparing P (M-PDA-EGDMA) / BN: dissolving a polymer P (M-PDA-EGDMA) into an ethyl acetate solution to obtain a polymer solution, adding a rod-like silver nanoparticle solution into the polymer solution, uniformly mixing, and forming a film by 3D printing to obtain a three-dimensional structure of the P (M-PDA-EGDMA) / BN; performing freeze drying to obtain three-dimensional porous fibers; the porous fibers are filled with high-heat-conductivity filler boron nitride nanoparticles, and the stretchable flexible polymer heat conduction material is prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a preparation technology of a stretchable flexible thermally conductive material, which is mainly used in electronic heat dissipation, high temperature management and equipment requiring flexible thermal conductivity, and belongs to the field of polymer functional composite materials. Background Art

[0002] The application of thermal conductive materials is crucial in electronic devices and high-tech fields. Traditional thermal conductive materials, such as metals (such as copper, aluminum) and ceramics (such as aluminum nitride, silicon nitride), although excellent in thermal conductivity, usually have high rigidity and lack flexibility, which limits their use in flexible electronic devices and other applications that require flexible adaptation to shape. This limitation is particularly prominent in the design of modern electronic devices, such as flexible displays, wearable devices and flexible circuit boards, which require materials to have not only high thermal conductivity, but also maintain good performance under various operating conditions such as bending, stretching or squeezing.

[0003] In recent years, as electronic devices have developed towards being thinner, lighter and more flexible, the demand for materials that are both thermally conductive and flexible has continued to increase. This demand has driven the research on new thermally conductive materials, especially those that have excellent flexibility and stretchability while maintaining high thermal conductivity. For example, flexible thermally conductive materials such as thermally conductive silicone and thermally conductive polymer composites have begun to appear and have solved this technical problem to a certain extent. However, these materials still face some challenges, such as stability in high temperature environments, uniformity of thermal conductivity, and performance degradation during long-term use.

[0004] Therefore, developing a new type of stretchable flexible thermal conductive material that can maintain high thermal conductivity while having excellent flexibility and durability has become an important direction of current technical research. This will not only help promote the technological progress of flexible electronic devices, but can also be applied to a wider range of fields, such as smart wearable devices, flexible sensors and high temperature management systems. Summary of the invention

[0005] The present invention provides a method for preparing a stretchable flexible thermal conductive material, wherein P(M-PDA-EGDMA) is used as a polymer substrate and boron nitride (BN) is used as a high thermal conductive filler to prepare a stretchable flexible thermal conductive material, which has excellent thermal conductivity and flexibility and can meet the high requirements of modern electronic equipment for material performance. The technical purpose of the present invention is achieved by the following technical solution.

[0006] A method for preparing a stretchable flexible thermally conductive material comprises the following steps:

[0007] 1) Synthesis of P(M-PDA-EGDMA): When the molar ratio of 3-methacryloyl dopamine M-PDA to ethylene glycol dimethacrylate EGDMA is 2:(4.5-5.5), EGDMA, M-PDA and an initiator are placed in a container of N,N-dimethylformamide DMF, argon is introduced into the mixture, and then the mixture is heated to 55-65° C. and stirred to polymerize to obtain a reaction mixture;

[0008] 2) Preparation of P(M-PDA-EGDMA) / BN: The polymer P(M-PDA-EGDMA) was dissolved in an ethyl acetate solution to obtain a polymer solution, to which a rod-shaped silver nanoparticle solution was added, and the mixture was mixed evenly. The three-dimensional structure was obtained by 3D printing. After freeze-drying, three-dimensional porous fibers were obtained. The porous fibers were filled with boron nitride nanoparticles, a high thermal conductivity filler, to prepare a stretchable flexible polymer thermal conductive material.

[0009] In step 1), the initiator may be aminocyanate ABCN or azobisisobutyronitrile AIBN.

[0010] In step 1), methanol is added to dilute the reaction mixture, and then ether is added to precipitate the polymer. The precipitation process is repeated 2-3 times to completely remove unreacted monomers and residual solvent.

[0011] The method is characterized in that the time for introducing argon in step 1) should be no less than 10 minutes.

[0012] The concentration of the polymer solution prepared in step 2) should be controlled at 0.6 g / mL to 1.2 g / mL.

[0013] In step 2), a rod-shaped silver nanoparticle solution with a mass fraction of 5% can be added to the polymer solution.

[0014] In step 2), freeze drying is performed at -70°C for 24 hours.

[0015] The present invention provides a method for preparing a stretchable flexible thermal conductive material, which achieves a combination of high thermal conductivity and excellent flexibility through precise material selection and optimized preparation process. This new material can meet the high requirements of modern electronic equipment for material performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is the preparation scheme of P(M-PDA-EGDMA).

[0017] Figure 2 The packing structure and preparation scheme. DETAILED DESCRIPTION

[0018] Two embodiments of the present invention are provided below to further illustrate the present invention, but not to limit the scope of the present invention.

[0019] Example 1

[0020] 1) Synthesis of P(M-PDA-EGDMA): EGDMA (6.5 g, 50 mmol), M-PDA (4.4 g, 20 mmol) and aminocyanate (ABCN) (152 mg, 0.92 mmol) were placed in a round-bottom flask containing 20 mL of N,N-dimethylformamide (DMF) at a molar ratio of 3-methacryloyl dopamine (M-PDA):ethylene glycol dimethacrylate (EGDMA) of 2:5, and argon was passed through the mixture for 10 min. The solution was heated to 60°C and stirred for 12 h for polymerization. Subsequently, 20 mL of methanol was added to dilute the reaction mixture, and then 200 mL of ether was added to precipitate the polymer. The precipitation process was repeated 2-3 times to completely remove the unreacted monomers and residual solvent.

[0021] 2) Preparation of P(M-PDA-EGDMA) / BN: 5g of polymer P(M-PDA-EGDMA) was fully dissolved in 20g of ethyl acetate solution to obtain a polymer solution with a mass fraction of 20%, and then 5g of rod-shaped silver nanoparticle solution (mass fraction of 5%) was added thereto and stirred at 25°C for 2h to form a uniform solution, and its three-dimensional structure was obtained by 3D printing. The principle of 3D printing film formation is based on the process of layer-by-layer deposition of materials. The printer deposits the solution or molten material onto the substrate layer by layer, forming each layer according to a preset path. After each layer is solidified, the next layer continues to be deposited, and finally a three-dimensional structure is formed. After standing for 1h, the hydrophobic phase and the hydrophilic solvent in the system will phase separate, which can achieve the effect of initial solvent removal. The residual solvent is removed by freeze drying at -70°C for 24h to obtain a three-dimensional porous fiber with uniform pore size. Then, the porous fiber is filled with high thermal conductivity filler boron nitride nanoparticles to prepare a stretchable flexible thermal conductive material.

[0022] Example 2

[0023] 1) Synthesis of P(M-PDA-EGDMA): EGDMA (6.5 g, 50 mmol), M-PDA (4.4 g, 20 mmol) and azobisisobutyronitrile (AIBN) (107 mg, 0.92 mmol) were placed in a round-bottom flask containing 20 mL of N,N-dimethylformamide (DMF) at a molar ratio of 2:5. Argon was passed through the mixture for 10 min. The solution was heated to 60 °C and stirred for 12 h for polymerization. Subsequently, 20 mL of methanol was added to dilute the reaction mixture, and then 200 mL of ether was added to precipitate the polymer. The precipitation process was repeated 2-3 times to completely remove the unreacted monomers and residual solvent.

[0024] 2) Preparation of P(M-PDA-EGDMA) / BN: 5g of polymer P(M-PDA-EGDMA) was fully dissolved in 20g of DMF to obtain a polymer solution with a mass fraction of 20%, to which a rod-shaped silver nanoparticle solution with a mass fraction of 5% was added and stirred at 25°C for 2h to form a uniform solution, and its three-dimensional structure was obtained by 3D printing. The principle of 3D printing film formation is based on the process of layer-by-layer deposition of materials. The printer deposits the solution or molten material onto the substrate layer by layer, forming each layer according to a preset path. After each layer is solidified, the next layer continues to be deposited, and finally a three-dimensional structure is formed. After standing for 1h, the hydrophobic phase and the hydrophilic solvent in the system will phase separate, which can achieve the effect of initial solvent removal. The residual solvent is removed by freeze drying at -70°C for 24h to obtain a three-dimensional porous fiber with uniform pore size. Then, the porous fiber is filled with high thermal conductivity filler boron nitride nanoparticles to prepare a stretchable flexible thermal conductive material.

[0025] The present invention is described above by way of example. It should be noted that, without departing from the core of the present invention, any simple deformation, modification or other equivalent replacement that can be made by those skilled in the art without inventive effort falls within the protection scope of the present invention.

Claims

1. A method for preparing a stretchable flexible thermally conductive material, comprising the following steps: 1) Synthesis of P(M-PDA-EGDMA): When the molar ratio of 3-methacryloyl dopamine M-PDA to ethylene glycol dimethacrylate EGDMA is 2:(4.5-5.5), EGDMA, M-PDA and an initiator are placed in a container of N,N-dimethylformamide DMF, argon is introduced into the mixture, and then the mixture is heated to 55-65° C. and stirred to polymerize to obtain a reaction mixture; 2) Preparation of P(M-PDA-EGDMA) / BN: The polymer P(M-PDA-EGDMA) was dissolved in an ethyl acetate solution to obtain a polymer solution, to which a rod-shaped silver nanoparticle solution was added, and the mixture was mixed evenly. The three-dimensional structure was obtained by 3D printing. After freeze-drying, three-dimensional porous fibers were obtained. The porous fibers were filled with boron nitride nanoparticles, a high thermal conductivity filler, to prepare a stretchable flexible polymer thermal conductive material.

2. The preparation method according to claim 1, characterized in that In step 1), the initiator is aminocyanate ABCN or azobisisobutyronitrile AIBN.

3. The preparation method according to claim 1, characterized in that In step 1), methanol is added to dilute the reaction mixture, and then diethyl ether is added to precipitate the polymer.

4. The preparation method according to claim 1, characterized in that The time for introducing argon in step 1) is 10 min.

5. The preparation method according to claim 1, characterized in that The concentration of the polymer solution prepared in step 2) is controlled at 0.6 g / mL to 1.2 g / mL.

6. The preparation method according to claim 1, characterized in that In step 2), a rod-shaped silver nanoparticle solution with a mass fraction of 5% is added to the polymer solution.

7. The preparation method according to claim 1, characterized in that In step 2), freeze-dry at -70°C for 24 h.

Citation Information

Patent Citations

  • Directionally arranged boron nitride-coated polydopamine-coated silver hybrid nanosheets flexible thermal interface material and preparation method of flexible thermal interface material

    CN113150544A

  • Enhanced hydrogel material for promoting tissue repair, hydrogel patch and preparation method

    CN117695438A