Antistatic environment-friendly automobile foot mat and preparation method thereof
By using TPE, modified resin and modified carbon fiber in automotive foot pad materials, a dense crosslinking network and composite structure is formed, which solves the problems of insufficient anti-static, waterproof and aging resistance of existing materials, and achieves high performance Car foot mat.
Patent Information
- Application Number
- CN202411259412.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing automotive foot pad materials have shortcomings in antistatic, waterproof and aging resistance, which cannot meet the market's demand for higher performance.
TPE material is used with modified resin and modified carbon fibers, and by forming a dense three-dimensional crosslinking network structure and composite structure, the uniformity and dispersion of the antistatic agent are enhanced, and the mechanical, waterproof and antistatic properties of the material are improved.
It significantly improves the anti-static, waterproof and aging resistance of automotive foot pads, while maintaining excellent mechanical and mechanical properties, meeting the market's demand for high-performance automotive foot pads.
Smart Images

Figure BDA0005035078940000201
Abstract
Description
Technical Field
[0001] The present application relates to the field of floor mat materials, and in particular to an antistatic and environmentally friendly automobile floor mat and a preparation method thereof. Background Art
[0002] With the development of the automobile industry, car floor mats, as an important part of car interior, not only provide comfortable feeling for drivers and passengers, but also protect the original carpet of the vehicle from wear and tear, prevent stains from penetrating into the car body and improve the cleanliness of the car interior.
[0003] In recent years, as consumers' pursuit of personalization and a higher quality of life has grown, a growing number of customized car floor mats have appeared on the market. These mats are precisely measured and designed according to specific vehicle models, allowing them to better conform to the contours of the vehicle floor, thereby enhancing stability and aesthetics. Furthermore, to further enhance the functionality and durability of these mats, the use of new materials has become a research and development focus.
[0004] Currently, common car floor mat materials on the market include rubber, PVC (polyvinyl chloride), and TPE (thermoplastic elastomer). Among them, TPE, a new environmentally friendly material, has emerged in the car floor mat field in recent years. It combines the ease of plastic processing with the elasticity of rubber, and has excellent wear and crack resistance. It is also non-toxic and odorless, meeting current consumer demand for car floor mat materials.
[0005] However, there are still some problems with the application of TPE materials in car floor mats. For example, the antistatic properties, waterproof properties, and aging resistance of TPE car floor mats need to be significantly improved to meet the higher consumer demand for existing car floor mats. Therefore, in order to solve the above problems, the present application provides an antistatic and environmentally friendly car floor mat and a preparation method thereof. The antistatic, waterproof, aging and oxidation resistance properties of the car floor mat can be significantly improved while maintaining excellent mechanical properties. The antistatic, waterproof, aging and oxidation resistance properties of the car floor mat are excellent in practical performance, meet the performance requirements of existing consumers for car floor mats, and have excellent market application value. Summary of the Invention
[0006] In order to solve the above problems, the first aspect of the present application provides an antistatic environmentally friendly car floor mat, which comprises, by weight, 60 to 75 parts of TPE, 15 to 25 parts of modified resin, 10 to 25 parts of functional resin, 3 to 5 parts of oil, 8 to 15 parts of antistatic agent, 6 to 10 parts of dispersant, 1 to 2 parts of coupling agent, and 10 to 20 parts of auxiliary agent.
[0007] As a preferred solution, the mass ratio of the TPE, modified resin and functional resin is (6.5-7.5): (2-2.5): (1.5-2).
[0008] As a preferred solution, the mass ratio of the TPE, modified resin and functional resin is (6.6-7): (2.2-2.4): (1.6-1.8).
[0009] As a preferred solution, the mass ratio of the modified resin to the antistatic agent is (2-2.5): (1-1.4).
[0010] As a preferred solution, the TPE is SEBS.
[0011] As a preferred solution, the weight average molecular weight of the SEBS is 60,000 to 150,000.
[0012] As a preferred solution, the SEBS is a composition of SEBS with a weight average molecular weight of 70,000 to 80,000 and SEBS with a weight average molecular weight of 120,000 to 140,000.
[0013] As a preferred solution, the mass ratio of the SEBS with a weight average molecular weight of 70,000 to 80,000 to the SEBS with a weight average molecular weight of 120,000 to 140,000 is (1.5 to 2): (4 to 5).
[0014] As a preferred solution, the preparation method of the modified resin includes the following steps: S1: adding acrylonitrile, glycidyl methacrylate and benzophenone into a reaction vessel and irradiating the reaction at a wavelength of 350 to 400 nm under nitrogen for 2 to 3 hours to obtain a prepolymer; S2: uniformly mixing the prepolymer, acrylamide, α-methylstyrene and N-vinylcaprolactam and adding the mixture to an acetone solvent, then adding benzoyl peroxide, heating the mixture to 75 to 85° C. and stirring the mixture in a closed container for 8 to 12 hours, adding triethanolamine to adjust the pH to 8 to 8.5, filtering the mixture and washing the product with deionized water to obtain a preproduct; S3: mixing the preproduct with succinic anhydride and 3-aminopropyltriethoxysilane, maintaining the temperature at 60 to 65° C. and reacting for 1.5 to 2 hours, filtering and washing the product after completion, and vacuum drying the mixture to obtain the preproduct.
[0015] As a preferred solution, the mass ratio of acrylonitrile, glycidyl methacrylate and benzophenone is (6-9): (2-3.5): (0.5-0.8).
[0016] As a preferred solution, the mass ratio of the prepolymer, acrylamide, α-methylstyrene and N-vinylcaprolactam is (8-11): (20-35): (2-4): (1-3).
[0017] As a preferred solution, the mass ratio of the prepolymer, acrylamide, α-methylstyrene and N-vinylcaprolactam is (9-10): (25-30): (2.5-3): (1-1.8).
[0018] As a preferred solution, the mass ratio of the pre-product to succinic anhydride and 3-aminopropyltriethoxysilane is (10-15): (2-3): (0.4-0.6).
[0019] The modified resin added in this application can effectively improve the mechanical properties of the car floor mats while greatly improving their antistatic, waterproof and aging resistance properties. First, the added modified resin carries multiple active groups that can greatly enhance the cross-linking reaction strength with the TPE base material, thereby forming a denser three-dimensional cross-linked network structure during the preparation of the foot pad material. The presence of this structure can significantly reduce the free rate of free groups and water molecules in the system after the materials are mixed and cured, reduce the contact frequency between them, and thus maintain excellent internal system extremely low reactivity and water molecule penetration resistance during long-term use; secondly, the added modified resin can effectively wrap the antistatic agent added in this application through good intermolecular interactions and hydrogen bonding during the preparation of the foot pad material, acting as an efficient compatible carrier for the antistatic agent particles in the entire preparation process, thereby greatly improving the uniformity of the antistatic particles in the foot pad material system, increasing the average length of the electron path, and significantly increasing the content of the antistatic agent particles on the foot pad surface, thereby significantly increasing the surface roughness and reducing the surface energy, not only having a good anti-slip effect, but also significantly reducing the formation rate of the hydration layer on the foot pad surface, significantly increasing the water molecule penetration resistance, and thus effectively helping to enhance the antistatic performance during long-term use while maintaining good mechanical and waterproof properties.
[0020] As a preferred solution, the functional resin is at least one of PVC resin, EVA resin, epoxy block resin or PC resin.
[0021] As a preferred solution, the functional resin is a composition of PVC resin and epoxy block resin.
[0022] As a preferred solution, the mass ratio of the PVC resin to the epoxy block resin is (5-5.5):(2-2.8).
[0023] As a preferred solution, the weight average molecular weight of the PVC resin is 60,000 to 80,000.
[0024] As a preferred solution, the weight average molecular weight of the epoxy block resin is 5,000 to 10,000.
[0025] As a preferred solution, the oil agent is naphthenic oil or epoxidized soybean oil.
[0026] As a preferred solution, the oil agent is epoxidized soybean oil.
[0027] As a preferred solution, the antistatic agent is modified carbon fiber.
[0028] As a preferred solution, the preparation method of the modified carbon fiber comprises the following steps: S1: adding titanium dioxide, succinic anhydride and zinc nitrate hexahydrate to a DMF solution, heating the mixture to 50-60°C and keeping the mixture warm for 40-60 minutes, adding a DMF solution of 2,5-dihydroxyterephthalic acid dropwise during the heat preservation period, heating the mixture to 80-85°C and keeping the mixture warm for 5-6 hours after the addition is completed; S2: adding the carbon fiber mixture to the DMF solvent, adding succinic anhydride and triisostearyl titanate isopropyl and heating the mixture to 60-70°C and keeping the mixture warm for reaction. 3 to 3.5 hours, after completion, filter, wash and take out to obtain pretreated carbon fiber; S3: add the pretreated carbon fiber to the reaction container of S1, heat it to 120 to 130 ° C, stir and react at 100 to 150 rpm for 28 to 35 hours, after the reaction is completed, filter and take out the product, add it to deionized water, heat it to 60 to 70 ° C and ultrasonically oscillate at 300 to 400 W power for 2 to 3 hours, then naturally cool to room temperature, centrifuge and filter, wash the product with deionized water and methanol in turn for 2 to 3 times, and vacuum dry it at 80 to 90 ° C to obtain it.
[0029] As a preferred solution, the mass ratio of titanium dioxide, succinic anhydride, zinc nitrate hexahydrate and 2,5-dihydroxyterephthalic acid is (0.6-0.8): (1.1-1.3): (1.4-1.8): (2.8-3.4).
[0030] As a preferred solution, the mass ratio of the carbon fiber, succinic anhydride and triisostearyl isopropyl titanate is (3-3.5): (1-1.5): (0.4-0.6).
[0031] As a preferred solution, the mass ratio of titanium dioxide to pretreated carbon fiber is (0.6-0.8): (5-5.5).
[0032] As a preferred solution, the average particle size of the titanium dioxide is 10 to 20 nm.
[0033] As a preferred solution, the average diameter of the carbon fibers is 6.5 to 8 μm; and the average length of the carbon fibers is 4 to 6 mm.
[0034] The modified carbon fiber antistatic agent particles added in the present application can effectively improve the mechanics, waterproof, anti-aging and antistatic properties of automobile mat materials. First, the more active sites and active groups that the modified carbon fiber particle surfaces added have can significantly enhance the binding connection force between itself and the system by the assistance of modified resin, not only can strengthen its dispersion in the system and the fixation after solidification, the composite particles of modified carbon fiber and its surface load can also form effective point-line support and connection structure when external force is applied, thus different from existing antistatic agent particles when external force is applied, it is possible to improve significant mechanics and mechanical property enhancement effect; secondly, the composite structure formed can significantly enhance the flow path length of electrons on carbon fiber, and the backtracking and countercurrent phenomenon of electrons can be significantly reduced by the aggregation of electrons and holes, and better dispersion effect forms a longer electron dissipation path connected to each other, electrons can be directly transported to the surface of automobile mat materials at high speed from material interior, significantly accelerate electron dissipation speed, avoid static accumulation, obtain excellent antistatic properties.
[0035] As a preferred solution, the dispersant is a combination of sodium dodecylbenzenesulfonate and carboxymethyl cellulose.
[0036] As a preferred solution, the mass ratio of sodium dodecylbenzenesulfonate to carboxymethyl cellulose is (4-5): (1-1.5).
[0037] As a preferred solution, the coupling agent is a titanate coupling agent or a silane coupling agent.
[0038] As a preferred solution, the coupling agent is a silane coupling agent.
[0039] As a preferred solution, the silane coupling agent is γ-aminopropyltriethoxysilane or γ-methacryloxypropyltrimethoxysilane.
[0040] As a preferred solution, the auxiliary agent at least includes a flame retardant, a brightener and an antioxidant.
[0041] As a preferred solution, the mass ratio of the flame retardant, brightener and antioxidant is (6-8): (2-3): (1-2).
[0042] As a preferred solution, the flame retardant is at least one phosphate flame retardant.
[0043] As a preferred solution, the flame retardant is tricresyl phosphate.
[0044] As a preferred solution, the brightener is polyethylene wax or polypropylene wax.
[0045] As a preferred solution, the antioxidant is at least one of antioxidant 1010, antioxidant 1076, antioxidant 168, and antioxidant 330.
[0046] The second aspect of the present application provides a preparation method of the above-mentioned antistatic environmentally friendly car floor mat, which specifically includes the following steps: S1: adding TPE, modified resin, functional resin, antistatic agent, dispersant, and additives to a high-speed mixer and stirring at a speed of 300-400 rpm for 40-60 minutes to mix evenly to obtain a premix; S2: adding the premix to a twin-screw extruder, and adding an oil agent and a coupling agent, controlling the heating temperature to 190-220°C, melt-mixing and extruding, and water-cooling and granulating at 50-60°C to obtain mixed particles; S3: sending the mixed particles into an injection molding machine, injecting them into a car floor mat mold at 180-200°C for molding, taking out the molded product after the injection molding is completed, and cooling it to 30-40°C. The molded product is trimmed, cleaned, and trimmed to size to obtain the product.
[0047] This application has the following beneficial effects:
[0048] 1. The antistatic and environmentally friendly car floor mat provided in this application can significantly improve the antistatic, waterproof, aging-resistant and oxidation-resistant properties of the car floor mat while maintaining excellent mechanical properties. It has excellent practical performance, meets the performance requirements of existing consumers for car floor mats, and has excellent market application value.
[0049] 2. The present application provides an antistatic and environmentally friendly car floor mat, in which the modified resin added carries multiple active groups that can greatly enhance the cross-linking reaction strength with the TPE base material, thereby forming a denser three-dimensional cross-linked network structure during the preparation of the floor mat material. The existence of this structure can greatly reduce the free speed of free groups and water molecules in the system after the materials are mixed and cured, reduce the contact frequency between them, and thus maintain excellent internal system extremely low reactivity and water molecule penetration resistance during long-term use.
[0050] 3. The present application provides an antistatic and environmentally friendly car floor mat. The modified resin added thereto can effectively wrap the antistatic agent added in the present application through good intermolecular interaction and hydrogen bonding during the preparation process of the floor mat material, and acts as an efficient compatible carrier of the antistatic agent particles in the entire preparation process, thereby greatly improving the uniformity of the antistatic particles in the floor mat material system, increasing the average length of the electron path, and being able to greatly increase the content of the antistatic agent particles on the floor mat surface, thereby greatly increasing the surface roughness and reducing the surface energy. It not only has a good anti-slip effect, but also can greatly reduce the formation speed of the hydration layer on the floor mat surface, greatly improve the water molecule penetration resistance, and obtain excellent waterproof performance.
[0051] 4. The antistatic and environmentally friendly car floor mat provided in the present application, the added modified carbon fiber antistatic agent particles can effectively improve the mechanical, waterproof, aging resistance and antistatic properties of the car floor mat material; the more active sites and active groups on the surface of the modified carbon fiber particles can greatly enhance the bonding connection between them and the system with the assistance of the modified resin, which can not only strengthen their dispersion in the system and the fixation after curing, but also provide fixed mechanical support and connection; on the other hand, the composite structure formed can greatly enhance the length of the flow path of electrons on the carbon fiber, and can greatly reduce the backtracking and backflow of electrons through the aggregation of electrons and holes, and the better dispersion effect forms a longer interconnected electron dissipation path, which can directly transport electrons from the inside of the material to the surface of the car floor mat material at high speed, greatly accelerating the electron dissipation speed, avoiding static electricity accumulation, and obtaining excellent antistatic properties. DETAILED DESCRIPTION
[0052] The following text further illustrates and demonstrates the technical solutions described in the above-mentioned summary of the invention in the form of specific implementation plans. The following examples are merely practical examples used to illustrate and explain the technical solutions in the specification and should not limit the scope of the claims to be protected by this application. All technical products based on the technical solutions described in the summary of the invention in this application should be included in the scope of protection to be protected by this application.
[0053] In the following examples, unless otherwise specified, the raw materials are all commercially available products or can be prepared by methods well known to those skilled in the art.
[0054] Example 1
[0055] Example 1 The first aspect provides an antistatic environmentally friendly car floor mat, which comprises, by mass, 68.5 parts of TPE, 23.8 parts of modified resin, 17.2 parts of functional resin, 4.2 parts of oil, 11.5 parts of antistatic agent, 7.2 parts of dispersant, 1.8 parts of coupling agent, and 12.5 parts of auxiliary agent.
[0056] The TPE is SEBS, which is a combination of SEBS with a weight-average molecular weight of 76,000 and SEBS with a weight-average molecular weight of 125,000, with a mass ratio of 1.6:4.4. The SEBS were purchased from Shanghai Yi Zeng Plasticization Co., Ltd., which sells products of corresponding molecular weights.
[0057] The functional resin is a combination of PVC resin and epoxy block resin, with a mass ratio of 5.4:2.6. The PVC resin has a weight-average molecular weight of 72,000 and was purchased from Shandong Guoheng New Materials Technology Co., Ltd.; the epoxy block resin has a weight-average molecular weight of 7,800 and was purchased from BASF as an L87 ethylene oxide-propylene oxide block copolymer.
[0058] The preparation method of the modified resin includes the following steps, calculated by mass: S1: adding 8.5 parts of acrylonitrile, 2.8 parts of glycidyl methacrylate and 0.76 parts of benzophenone to a reaction container, irradiating the reaction at a wavelength of 380 nm under nitrogen for 2.5 hours to obtain a prepolymer; S2: uniformly mixing 9.2 parts of the prepolymer, 28.5 parts of acrylamide, 2.6 parts of α-methylstyrene and 1.5 parts of N-vinylcaprolactam, adding the mixture to 200 parts of acetone solvent, then adding 0.21 parts of benzoyl peroxide, heating the mixture to 80°C, sealing the mixture with stirring and reacting for 9.5 hours, adding triethanolamine to adjust the pH to 8.2, filtering the mixture and washing the product with deionized water to obtain a preproduct; S3: mixing 13.8 parts of the preproduct with 2.2 parts of succinic anhydride and 0.54 parts of 3-aminopropyltriethoxysilane, maintaining the temperature at 60°C for 1.5 hours, filtering and washing the product after completion, and drying the mixture in a vacuum oven at 75°C to obtain the preproduct.
[0059] The oil agent is epoxidized soybean oil, which is an industrial high-purity product purchased from Shandong Shengqi New Materials Co., Ltd.
[0060] The antistatic agent is modified carbon fiber; the preparation method of the modified carbon fiber comprises the following steps, calculated by mass: S1: adding 0.74 parts of titanium dioxide, 1.25 parts of succinic anhydride and 1.55 parts of zinc nitrate hexahydrate to 80 parts of DMF solution, heating to 60°C and keeping warm for 50 minutes, adding 3.2 parts of 2,5-dihydroxyterephthalic acid DMF solution (25 parts in total) dropwise during the keeping warm period, heating to 85°C after the addition is completed and keeping warm for 5.5 hours; S2: adding 3.4 parts of carbon fiber to 80 parts of DMF solvent, adding 1.4 parts of succinic anhydride, and keeping warm for 5.5 hours; The dianhydride and 0.52 parts of isopropyl triisostearyl titanate were heated to 65°C and kept warm for 3 hours. After completion, the product was filtered, washed and taken out to obtain pretreated carbon fiber; S3: 5.2 parts of pretreated carbon fiber were added to the reaction vessel of S1, heated to 130°C, stirred at 120rpm for 29 hours, and after completion of the reaction, the product was filtered out, added to deionized water, heated to 65°C and ultrasonically vibrated at 400W power for 2 hours, then naturally cooled to room temperature, centrifuged and filtered, and the product was washed with deionized water and methanol for 3 times, and vacuum dried at 85°C to obtain the product.
[0061] The average particle size of titanium dioxide is 14.8 nm; the average diameter of carbon fiber is 6.8 μm, and the average length of carbon fiber is 5.5 mm, and products of corresponding sizes were purchased from Shanghai Lishuo Composite Materials Technology Co., Ltd.
[0062] The dispersant is a composition of sodium dodecylbenzenesulfonate and carboxymethyl cellulose, and the mass ratio of the two is 4.5:1.2.
[0063] The coupling agent is γ-aminopropyltriethoxysilane.
[0064] The auxiliary agent is a composition of a flame retardant, a brightener and an antioxidant, and the mass ratio of the three is 8:3:1.5.
[0065] The flame retardant is tricresyl phosphate; the brightener is polyethylene wax, purchased from Dongguan Dingxin Plastic Raw Materials Co., Ltd., model LA-B10 product; and the antioxidant is antioxidant 1076.
[0066] A second aspect of this embodiment provides a method for preparing the above-mentioned antistatic and environmentally friendly car floor mats, which specifically includes the following steps: S1: adding TPE, modified resin, functional resin, antistatic agent, dispersant, and additives to a high-speed mixer and stirring at 350 rpm for 55 minutes to mix evenly to obtain a premix; S2: adding the premix to a twin-screw extruder, and adding an oil agent and a coupling agent, controlling the heating temperature to 210°C, melt-mixing and extruding, and water-cooling and granulating at 58°C to obtain mixed pellets; S3: sending the mixed pellets to an injection molding machine, injecting them into a car floor mat mold at 200°C for molding, taking out the molded product after the injection molding is completed, cooling it to 35°C, and trimming, cleaning, and trimming the molded product to obtain the product.
[0067] Example 2
[0068] Example 2 The first aspect provides an antistatic environmentally friendly car floor mat, which is composed of the following raw materials, in parts by mass: 75 parts of TPE, 20 parts of modified resin, 15.5 parts of functional resin, 3.5 parts of oil, 10.2 parts of antistatic agent, 7.2 parts of dispersant, 1.8 parts of coupling agent, and 12.5 parts of auxiliary agent.
[0069] The TPE is SEBS, which is a combination of SEBS with a weight average molecular weight of 76,000 and SEBS with a weight average molecular weight of 125,000, with a mass ratio of 2:4. The SEBS were purchased from Shanghai Yi Zeng Plasticization Co., Ltd., which sells products of corresponding molecular weights.
[0070] The functional resin is a combination of PVC resin and epoxy block resin, with a mass ratio of 5:2.8. The PVC resin has a weight-average molecular weight of 72,000 and was purchased from Shandong Guoheng New Materials Technology Co., Ltd.; the epoxy block resin has a weight-average molecular weight of 7,800 and was purchased from BASF as an L87 ethylene oxide-propylene oxide block copolymer.
[0071] The preparation method of the modified resin includes the following steps, calculated by mass: S1: adding 8.5 parts of acrylonitrile, 2.8 parts of glycidyl methacrylate and 0.76 parts of benzophenone to a reaction container, irradiating the reaction at a wavelength of 380 nm under nitrogen for 2.5 hours to obtain a prepolymer; S2: uniformly mixing 9.2 parts of the prepolymer, 28.5 parts of acrylamide, 2.6 parts of α-methylstyrene and 1.5 parts of N-vinylcaprolactam, adding the mixture to 200 parts of acetone solvent, then adding 0.21 parts of benzoyl peroxide, heating the mixture to 80°C, sealing the mixture with stirring and reacting for 9.5 hours, adding triethanolamine to adjust the pH to 8.2, filtering the mixture and washing the product with deionized water to obtain a preproduct; S3: mixing 13.8 parts of the preproduct with 2.2 parts of succinic anhydride and 0.54 parts of 3-aminopropyltriethoxysilane, maintaining the temperature at 60°C for 1.5 hours, filtering and washing the product after completion, and drying the mixture in a vacuum oven at 75°C to obtain the preproduct.
[0072] The oil agent is epoxidized soybean oil, which is an industrial high-purity product purchased from Shandong Shengqi New Materials Co., Ltd.
[0073] The antistatic agent is modified carbon fiber; the preparation method of the modified carbon fiber comprises the following steps, calculated by mass: S1: adding 0.74 parts of titanium dioxide, 1.25 parts of succinic anhydride and 1.55 parts of zinc nitrate hexahydrate to 80 parts of DMF solution, heating to 60°C and keeping warm for 50 minutes, adding 3.2 parts of 2,5-dihydroxyterephthalic acid DMF solution (25 parts in total) dropwise during the keeping warm period, heating to 85°C after the addition is completed and keeping warm for 5.5 hours; S2: adding 3.4 parts of carbon fiber to 80 parts of DMF solvent, adding 1.4 parts of succinic anhydride, and keeping warm for 5.5 hours; The dianhydride and 0.52 parts of isopropyl triisostearyl titanate were heated to 65°C and kept warm for 3 hours. After completion, the product was filtered, washed and taken out to obtain pretreated carbon fiber; S3: 5.2 parts of pretreated carbon fiber were added to the reaction vessel of S1, heated to 130°C, stirred at 120rpm for 29 hours, and after completion of the reaction, the product was filtered out, added to deionized water, heated to 65°C and ultrasonically vibrated at 400W power for 2 hours, then naturally cooled to room temperature, centrifuged and filtered, and the product was washed with deionized water and methanol for 3 times, and vacuum dried at 85°C to obtain the product.
[0074] The average particle size of titanium dioxide is 14.8 nm; the average diameter of carbon fiber is 6.8 μm, and the average length of carbon fiber is 5.5 mm, and products of corresponding sizes were purchased from Shanghai Lishuo Composite Materials Technology Co., Ltd.
[0075] The dispersant is a composition of sodium dodecylbenzenesulfonate and carboxymethyl cellulose, and the mass ratio of the two is 4.5:1.2.
[0076] The coupling agent is γ-aminopropyltriethoxysilane.
[0077] The auxiliary agent is a composition of a flame retardant, a brightener and an antioxidant, and the mass ratio of the three is 8:3:1.5.
[0078] The flame retardant is tricresyl phosphate; the brightener is polyethylene wax, purchased from Dongguan Dingxin Plastic Raw Materials Co., Ltd., model LA-B10 product; and the antioxidant is antioxidant 1076.
[0079] A second aspect of this embodiment provides a method for preparing the above-mentioned antistatic and environmentally friendly car floor mats, which specifically includes the following steps: S1: adding TPE, modified resin, functional resin, antistatic agent, dispersant, and additives to a high-speed mixer and stirring at 350 rpm for 55 minutes to mix evenly to obtain a premix; S2: adding the premix to a twin-screw extruder, and adding an oil agent and a coupling agent, controlling the heating temperature to 210°C, melt-mixing and extruding, and water-cooling and granulating at 58°C to obtain mixed pellets; S3: sending the mixed pellets to an injection molding machine, injecting them into a car floor mat mold at 200°C for molding, taking out the molded product after the injection molding is completed, cooling it to 35°C, and trimming, cleaning, and trimming the molded product to obtain the product.
[0080] Example 3
[0081] Example 3 The first aspect provides an antistatic environmentally friendly car floor mat, which is composed of the following raw materials, in parts by mass: 65 parts of TPE, 25 parts of modified resin, 20 parts of functional resin, 4.8 parts of oil, 13.2 parts of antistatic agent, 8.5 parts of dispersant, 1.8 parts of coupling agent, and 10 parts of auxiliary agent.
[0082] The TPE is SEBS, which is a combination of SEBS with a weight-average molecular weight of 76,000 and SEBS with a weight-average molecular weight of 125,000, with a mass ratio of 1.6:4.4. The SEBS were purchased from Shanghai Yi Zeng Plasticization Co., Ltd., which sells products of corresponding molecular weights.
[0083] The functional resin is a combination of PVC resin and epoxy block resin, with a mass ratio of 5.4:2.6. The PVC resin has a weight-average molecular weight of 72,000 and was purchased from Shandong Guoheng New Materials Technology Co., Ltd.; the epoxy block resin has a weight-average molecular weight of 7,800 and was purchased from BASF as an L87 ethylene oxide-propylene oxide block copolymer.
[0084] The preparation method of the modified resin includes the following steps, calculated by mass: S1: adding 8.5 parts of acrylonitrile, 2.8 parts of glycidyl methacrylate and 0.76 parts of benzophenone to a reaction container, irradiating the reaction at a wavelength of 380 nm under nitrogen for 2.5 hours to obtain a prepolymer; S2: uniformly mixing 9.2 parts of the prepolymer, 28.5 parts of acrylamide, 2.6 parts of α-methylstyrene and 1.5 parts of N-vinylcaprolactam, adding the mixture to 200 parts of acetone solvent, then adding 0.21 parts of benzoyl peroxide, heating the mixture to 80°C, sealing the mixture with stirring and reacting for 9.5 hours, adding triethanolamine to adjust the pH to 8.2, filtering the mixture and washing the product with deionized water to obtain a preproduct; S3: mixing 13.8 parts of the preproduct with 2.2 parts of succinic anhydride and 0.54 parts of 3-aminopropyltriethoxysilane, maintaining the temperature at 60°C for 1.5 hours, filtering and washing the product after completion, and drying the mixture in a vacuum oven at 75°C to obtain the preproduct.
[0085] The oil agent is epoxidized soybean oil, which is an industrial high-purity product purchased from Shandong Shengqi New Materials Co., Ltd.
[0086] The antistatic agent is modified carbon fiber; the preparation method of the modified carbon fiber comprises the following steps, calculated by mass: S1: adding 0.74 parts of titanium dioxide, 1.25 parts of succinic anhydride and 1.55 parts of zinc nitrate hexahydrate to 80 parts of DMF solution, heating to 60°C and keeping warm for 50 minutes, adding 3.2 parts of 2,5-dihydroxyterephthalic acid DMF solution (25 parts in total) dropwise during the keeping warm period, heating to 85°C after the addition is completed and keeping warm for 5.5 hours; S2: adding 3.4 parts of carbon fiber to 80 parts of DMF solvent, adding 1.4 parts of succinic anhydride, and keeping warm for 5.5 hours; The dianhydride and 0.52 parts of isopropyl triisostearyl titanate were heated to 65°C and kept warm for 3 hours. After completion, the product was filtered, washed and taken out to obtain pretreated carbon fiber; S3: 5.2 parts of pretreated carbon fiber were added to the reaction vessel of S1, heated to 130°C, stirred at 120rpm for 29 hours, and after completion of the reaction, the product was filtered out, added to deionized water, heated to 65°C and ultrasonically vibrated at 400W power for 2 hours, then naturally cooled to room temperature, centrifuged and filtered, and the product was washed with deionized water and methanol for 3 times, and vacuum dried at 85°C to obtain the product.
[0087] The average particle size of titanium dioxide is 14.8 nm; the average diameter of carbon fiber is 6.8 μm, and the average length of carbon fiber is 5.5 mm, and products of corresponding sizes were purchased from Shanghai Lishuo Composite Materials Technology Co., Ltd.
[0088] The dispersant is a composition of sodium dodecylbenzenesulfonate and carboxymethyl cellulose, and the mass ratio of the two is 5:1.
[0089] The coupling agent is γ-aminopropyltriethoxysilane.
[0090] The auxiliary agent is a combination of a flame retardant, a brightener and an antioxidant, and the mass ratio of the three is 7:2:1.
[0091] The flame retardant is tricresyl phosphate; the brightener is polyethylene wax, purchased from Dongguan Dingxin Plastic Raw Materials Co., Ltd., model LA-B10 product; and the antioxidant is antioxidant 1076.
[0092] A second aspect of this embodiment provides a method for preparing the above-mentioned antistatic and environmentally friendly car floor mats, which specifically includes the following steps: S1: adding TPE, modified resin, functional resin, antistatic agent, dispersant, and additives to a high-speed mixer and stirring at 350 rpm for 55 minutes to mix evenly to obtain a premix; S2: adding the premix to a twin-screw extruder, and adding an oil agent and a coupling agent, controlling the heating temperature to 210°C, melt-mixing and extruding, and water-cooling and granulating at 58°C to obtain mixed pellets; S3: sending the mixed pellets to an injection molding machine, injecting them into a car floor mat mold at 200°C for molding, taking out the molded product after the injection molding is completed, cooling it to 35°C, and trimming, cleaning, and trimming the molded product to obtain the product.
[0093] Comparative Example 1
[0094] The specific implementation of this comparative example is basically the same as that of Example 1, except that: the antistatic environmentally friendly car floor mat, in parts by mass, the raw materials are: 85.5 parts of TPE, 8.5 parts of modified resin, 24.5 parts of functional resin, 4.2 parts of oil, 16.8 parts of antistatic agent, 7.2 parts of dispersant, 1.8 parts of coupling agent, and 12.5 parts of additives.
[0095] Comparative Example 2
[0096] The specific implementation of this comparative example is basically the same as that of Example 1, except that: the antistatic environmentally friendly car floor mat, in parts by mass, the raw materials are: 70.5 parts of TPE, 33.5 parts of modified resin, 10.2 parts of functional resin, 4.2 parts of oil, 5.2 parts of antistatic agent, 7.2 parts of dispersant, 1.8 parts of coupling agent, and 12.5 parts of additives.
[0097] Comparative Example 3
[0098] The specific implementation of this comparative example is basically the same as that of Example 1, except that TPE is SEBS, and SEBS is a composition of SEBS with a weight average molecular weight of 76,000 and SEBS with a weight average molecular weight of 125,000, and the mass ratio of the two is 3.5:2.2.
[0099] Comparative Example 4
[0100] The specific implementation of this comparative example is basically the same as that of Example 1, except that the preparation method of the modified resin comprises the following steps, calculated in parts by mass: S1: adding 14.5 parts of acrylonitrile, 1.2 parts of glycidyl methacrylate and 0.32 parts of benzophenone into a reaction vessel and irradiating the reaction vessel under nitrogen at a wavelength of 380 nm for 2.5 hours to obtain a prepolymer; S2: adding 9.2 parts of prepolymer, 28.5 parts of acrylamide, 2.6 parts of α-methylstyrene and 1.5 parts of N-vinyl hexane to a prepolymer; The lactams were evenly mixed and added to 200 parts of acetone solvent, followed by adding 0.21 parts of benzoyl peroxide, and the temperature was raised to 80°C and the mixture was stirred in a closed manner for 9.5 hours. Triethanolamine was added to adjust the pH to 8.2, and then the product was filtered and washed with deionized water to obtain a pre-product; S3: 13.8 parts of the pre-product were mixed with 2.2 parts of succinic anhydride and 0.54 parts of 3-aminopropyltriethoxysilane, and the temperature was maintained at 60°C for 1.5 hours. After completion, the product was filtered and washed, and then vacuum-dried at 75°C to obtain the product.
[0101] Comparative Example 5
[0102] The specific implementation of this comparative example is basically the same as that of Example 1, except that the preparation method of the modified resin comprises the following steps, calculated in parts by mass: S1: adding 8.5 parts of acrylonitrile, 2.8 parts of glycidyl methacrylate and 0.76 parts of benzophenone into a reaction vessel and irradiating the vessel with a wavelength of 380 nm under nitrogen for 2.5 hours to obtain a prepolymer; S2: adding 5.5 parts of prepolymer, 38.5 parts of acrylamide, 1.5 parts of α-methylstyrene and 0.8 parts of N-vinyl hexane to a prepolymer; The lactams were evenly mixed and added to 240 parts of acetone solvent, followed by adding 0.24 parts of benzoyl peroxide, and the temperature was raised to 80°C and the mixture was stirred in a closed manner for 10 hours. Triethanolamine was added to adjust the pH to 8.4, and then the product was filtered and washed with deionized water to obtain a pre-product; S3: 13.8 parts of the pre-product were mixed with 2.2 parts of succinic anhydride and 0.54 parts of 3-aminopropyltriethoxysilane, and the temperature was maintained at 60°C for 1.5 hours. After completion, the product was filtered and washed, and then vacuum-dried at 75°C to obtain the product.
[0103] Comparative Example 6
[0104] The specific implementation of this comparative example is basically the same as that of Example 1, except that: the preparation method of the modified carbon fiber comprises the following steps, calculated in parts by mass: S1: 0.25 parts of titanium dioxide, 1.25 parts of succinic anhydride and 2.5 parts of zinc nitrate hexahydrate are mixed and added to 80 parts of DMF solution, the temperature is raised to 60°C and kept warm for 50 minutes, 5.5 parts of 2,5-dihydroxyterephthalic acid DMF solution (35 parts in total) are added dropwise during the insulation period, and after the addition is completed, the temperature is raised to 85°C and kept warm for 5.5 hours; S2: 3.4 parts of carbon fiber are mixed and added to 80 parts of DMF solvent. , add 1.4 parts of succinic anhydride and 0.52 parts of triisostearyl titanate isopropyl and heat to 65℃ for reaction for 3h. After completion, filter, wash and take out to obtain pretreated carbon fiber; S3: add 5.2 parts of pretreated carbon fiber to the reaction container of S1, heat to 130℃, stir at 120rpm for reaction 29h, after completion of the reaction, filter and take out the product, add it to deionized water, heat to 65℃ and ultrasonically vibrate at 400W power for 2h, then cool naturally to room temperature, centrifuge and wash the product with deionized water and methanol for 3 times, and vacuum dry at 85℃ to obtain it.
[0105] Comparative Example 7
[0106] The specific implementation of this comparative example is basically the same as that of Example 1, except that: the preparation method of the modified carbon fiber comprises the following steps, calculated in parts by mass: S1: 0.74 parts of titanium dioxide, 1.25 parts of succinic anhydride and 1.55 parts of zinc nitrate hexahydrate are mixed and added to 80 parts of DMF solution, the temperature is raised to 60°C and kept warm for 50 minutes, 3.2 parts of 2,5-dihydroxyterephthalic acid DMF solution (a total of 25 parts) are added dropwise during the insulation period, and after the addition is completed, the temperature is raised to 85°C and kept warm for 5.5 hours; S2: 5.8 parts of carbon fiber are mixed and added to 80 parts of DMF solvent , add 0.85 parts of succinic anhydride and 0.22 parts of triisostearyl titanate isopropyl and heat to 65℃ for reaction for 3 hours. After completion, filter, wash and take out to obtain pretreated carbon fiber; S3: add 3.5 parts of pretreated carbon fiber to the reaction container of S1, heat to 130℃, stir at 120rpm for reaction 26 hours, after the reaction is completed, filter and take out the product, add it to deionized water, heat to 65℃ and ultrasonically vibrate at 400W power for 2 hours, then cool naturally to room temperature, centrifuge and wash the product with deionized water and methanol for 3 times, and vacuum dry at 85℃ to obtain it.
[0107] Comparative Example 8
[0108] The specific implementation of this comparative example is basically the same as that of Example 1, except that: the average particle size of titanium dioxide is 38.5 nm, the average diameter of carbon fiber is 12.2 μm; the average length of the carbon fiber is 11.5 mm, and the corresponding size products are purchased from Shanghai Lishuo Composite Materials Technology Co., Ltd.
[0109] Performance evaluation
[0110] Antistatic performance: The surface resistance of the automobile floor mat materials prepared in the examples and comparative examples was tested using a surface resistivity meter. The test values were averaged over 10 tests and recorded in Table 1.
[0111] Mechanical properties: The tensile strength and elongation at break of the automobile floor mat materials prepared in the examples and comparative examples were tested with reference to standard GB / T 1039-92. The test values were averaged over 10 tests and recorded in Table 1.
[0112] Waterproof performance: The moisture permeability of the automobile floor mat materials prepared in the examples and comparative examples was tested with reference to the standard GB / T 16925-2008. The test values were recorded in Table 1 as the average value of 10 tests.
[0113] Aging resistance: The car floor mat materials prepared in the examples and comparative examples were prepared into 5 cm × 5 cm × 0.5 cm samples and placed in a constant temperature and humidity chamber at 60°C and 80% relative humidity for 120 hours. After 120 hours, the samples were taken out and naturally cooled to room temperature. The samples were observed to see if there was obvious curling, oxidation yellowing, or cracking. If so, they were marked as unqualified, otherwise they were qualified. 50 samples were tested in each group, and the qualified rate was recorded in Table 1.
[0114] Table 1 Performance test results
[0115]
[0116] It can be seen from the examples and comparative examples of the present application and the data results in Table 1 that Examples 1 to 3 of the present application have obvious advantages over comparative examples 1 to 8 in terms of mechanical properties, waterproof properties, antistatic properties and aging resistance. This is mainly because the modified resin and modified carbon fiber added in the present application are the result of the combined effect of other matching schemes, while comparative examples 1 to 8 did not adopt the technical scheme defined in the present application, resulting in obvious disadvantages in the above performance tests. This further proves the necessity of the technical scheme defined in the present application for the technical effect of the present application and solving technical problems.
Claims
1. An anti-static and environmentally friendly car mat, Features: In parts by mass, the raw materials are: 60-75 parts of TPE, 15-25 parts of modified resin, 10-25 parts of functional resin, 3-5 parts of oil agent, 8-15 parts of antistatic agent, 6-10 parts of dispersant, 1-2 parts of coupling agent, and 10-20 parts of auxiliary agent; The mass ratio of the TPE, modified resin and functional resin is (6.5-7.5): (2-2.5): (1.5-2); The mass ratio of the modified resin to the antistatic agent is (2-2.5): (1-1.4); Preparation method of the modified resin The following steps are involved: S1: Add acrylonitrile, glycidyl methacrylate and benzophenone into a reaction container and irradiate with a wavelength of 350-400nm under nitrogen for 2-3 hours to obtain a prepolymer; S2: Mix the prepolymer, acrylamide, α-methylstyrene and N-vinyl caprolactam evenly and add them to an acetone solvent, then add benzoyl peroxide, heat to 75-85°C, stir in a closed manner for 8-12 hours, add triethanolamine to adjust the pH to 8-8.5, then filter and wash the product with deionized water to obtain a pre-product; S3: Mix the pre-product with succinic anhydride and 3-aminopropyltriethoxysilane, keep the temperature at 60-65°C for 1.5-2 hours, and after completion, filter and wash the product, and vacuum dry it to obtain; The mass ratio of acrylonitrile, glycidyl methacrylate and benzophenone is (6-9): (2-3.5): (0.5-0.8); The mass ratio of the prepolymer, acrylamide, α-methylstyrene and N-vinylcaprolactam is (8-11): (20-35): (2-4): (1-3); The mass ratio of the pre-product to succinic anhydride and 3-aminopropyltriethoxysilane is (10-15): (2-3): (0.4-0.6); The functional resin is at least one of PVC resin, EVA resin, epoxy block resin or PC resin; The oil agent is naphthenic oil or epoxidized soybean oil; The antistatic agent is modified carbon fiber; As a preferred solution, the dispersant is a composition of sodium dodecylbenzene sulfonate and carboxymethyl cellulose; the mass ratio of the sodium dodecylbenzene sulfonate to the carboxymethyl cellulose is (4-5): (1-1.5); The coupling agent is a titanate coupling agent or a silane coupling agent.
2. The antistatic environmentally friendly car mat according to claim 1, Features: The TPE is SEBS; the weight average molecular weight of the SEBS is 60,000 to 150,000.
3. The antistatic environmentally friendly car mat according to claim 2, Features: The SEBS is a composition of SEBS with a weight average molecular weight of 70,000-80,000 and SEBS with a weight average molecular weight of 120,000-140,000; the mass ratio of SEBS with a weight average molecular weight of 70,000-80,000 and SEBS with a weight average molecular weight of 120,000-140,000 is (1.5-2):(4-5).
4. The antistatic environmentally friendly car mat according to claim 3, Features: The functional resin is a composition of PVC resin and epoxy block resin; the mass ratio of the PVC resin to the epoxy block resin is (5-5.5): (2-2.8).
5. The antistatic environmentally friendly car mat according to claim 4, Features: The weight average molecular weight of the PVC resin is 60,000 to 80,000.
6. The antistatic environmentally friendly car mat according to claim 5, Features: The weight average molecular weight of the epoxy block resin is 5,000 to 10,000.
7. The antistatic environmentally friendly car mat according to claim 6, Features: Preparation method of modified carbon fiber The following steps are involved: S1: titanium dioxide, succinic anhydride and zinc nitrate hexahydrate are mixed and added to a DMF solution, and the temperature is raised to 50-60°C and kept warm for 40-60 minutes. During the warming period, a DMF solution of 2,5-dihydroxyterephthalic acid is added dropwise, and after the addition is completed, the temperature is raised to 80-85°C and kept warm for 5-6 hours; S2: carbon fiber is mixed and added to a DMF solvent, succinic anhydride and triisostearyl titanate isopropyl are added, and the temperature is raised to 60-70°C and kept warm for 3-3.5 hours. After completion, the carbon fiber is filtered, washed and taken out to obtain a pretreated carbon fiber; S3: Add the pretreated carbon fiber to the reaction container of S1, heat it to 120-130°C, stir it at 100-150rpm for 28-35h, filter and take out the product after the reaction is completed, add it into deionized water, heat it to 60-70°C, and ultrasonically oscillate it at 300-400W for 2-3h, then naturally cool it to room temperature, centrifuge and filter it, wash the product with deionized water and methanol for 2-3 times, and dry it in a vacuum at 80-90°C to obtain the product.
8. The antistatic environmentally friendly car mat according to claim 7, Features: The mass ratio of the titanium dioxide, succinic anhydride, zinc nitrate hexahydrate and 2,5-dihydroxyterephthalic acid is (0.6-0.8): (1.1-1.3): (1.4-1.8): (2.8-3.4); the mass ratio of the titanium dioxide and the pretreated carbon fiber is (0.6-0.8): (5-5.5).
9. The antistatic environmentally friendly car mat according to claim 8, Features: The auxiliary agent at least includes a flame retardant, a brightener and an antioxidant; the mass ratio of the flame retardant, the brightener and the antioxidant is (6-8): (2-3): (1-2).
10. A method for preparing the antistatic and environmentally friendly car mat according to any one of claims 1 to 9, Features: The specific steps include: S1: Add TPE, modified resin, functional resin, antistatic agent, dispersant and additives into a high-speed mixer, stir at 300-400 rpm for 40-60 min to mix evenly, and obtain a premix; S2: Add the premix into a twin-screw extruder, add oil and coupling agent, control the heating temperature to 190-220°C, melt-mix and extrude, and water-cool at 50-60°C to obtain mixed pellets; S3: Send the mixed pellets into an injection molding machine, inject them into a car mat mold at 180-200°C for molding, take out the molded product after the injection molding is completed, cool it to 30-40°C, and trim the molded product to obtain the product.
Citation Information
Patent Citations
Environmentally-friendly car foot mat material and preparation method thereof
CN109651834A
Antibacterial odorless TPE (thermoplastic elastomer) for new energy automobile foot mat and preparation method of antibacterial odorless TPE
CN116987394A
Pressure-resistant shell high polymer material for LED lamp and preparation method of pressure-resistant shell high polymer material
CN118562291A
Composition for floor mat for automobile and method ofmaking the same
KR1020050055439A
Cited By
Epoxy resin coating resistant to chemical corrosion and preparation method thereof
CN119264785A