Glass fiber reinforced plastic composite board for aviation and preparation method of glass fiber reinforced plastic composite board

By optimizing the material composition and manufacturing process of fiberglass composite panels for aviation, using special fibers and resin matrices, and combining them with spraying additives, the problem of the composite panels' sensitivity to the environment and humidity has been solved, enabling high-performance applications in harsh environments.

CN118994839AInactive Publication Date: 2024-11-22ZHEJIANG XIZI AIRCRAFT COMPONENTS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411473669.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-22
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing fiberglass composite panels for aviation are sensitive to the environment and humidity. Long-term exposure to harsh environments may lead to performance degradation, and the manufacturing process is complex and difficult to control.

Method used

Special alkali-free glass fiber, R-grade high-strength glass fiber, silicon carbide fiber and zirconium oxide fiber are used as high-performance fibers, combined with organosilicon resin, furan resin and polyesterimide resin as resin matrix, and flame retardant, toughening agent, stabilizer and microwave absorber are sprayed to optimize the manufacturing process to improve the fire resistance, toughness, stability and microwave absorption performance of composite panels.

Benefits of technology

It improves the environmental adaptability of composite panels, enabling long-term use in harsh environments, solves the problem of sensitivity to environment and humidity, and enhances fire resistance, toughness and wave absorption performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994839A_ABST
    Figure CN118994839A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of composite board manufacturing, and discloses an aviation glass fiber reinforced plastic composite board and a preparation method thereof.The board is composed of high-performance fibers, a resin matrix and an additive, and special alkali-free glass fibers, R-grade high-strength glass fibers, silicon carbide fibers and zirconium oxide fibers are mixed according to the raw material proportion; the preparation method comprises the following steps: mixing organic silicon resin, furan resin and polyesterimide resin according to a raw material ratio, forming a pre-impregnated material from the two combined raw materials, heating and forming, then spraying a mixed preparation consisting of a flame retardant, a flexibilizer and a stabilizer, and finally spraying a wave-absorbing agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite plate manufacturing, in particular to a glass fiber reinforced plastic composite plate for aviation and a preparation method thereof. Background Art

[0002] FRP composite panels for aviation play an important role in the aerospace field with their unique advantages. This material is composed of glass fiber and resin matrix, and has the advantages of light weight, high strength, and corrosion resistance. It can effectively reduce the weight of aircraft structures, improve fuel efficiency, and enhance the durability and reliability of structures. With the continuous advancement of technology, the manufacturing process and performance of FRP composite panels for aviation have been significantly improved, making them more widely used in the aerospace field.

[0003] However, the defects of the existing technology cannot be ignored. Composite panels are sensitive to the environment and humidity, and long-term exposure to harsh environments may lead to performance degradation. This is mainly because the resin matrix in the composite panel is easily corroded by moisture, causing changes in the internal structure of the material, thereby affecting its mechanical properties and durability. In addition, the manufacturing process of composite panels is complicated, requiring precise control of the ratio and distribution of the resin matrix and reinforcing fibers, as well as factors such as temperature, pressure and time during the curing process, otherwise defects are prone to occur.

[0004] To overcome these drawbacks, future research should focus on improving the design of composite sheets, optimizing manufacturing processes, increasing the efficiency and accuracy of nondestructive testing techniques, and developing more economical and environmentally friendly materials. Summary of the invention

[0005] 1. Technical issues to be resolved In view of the deficiencies of the prior art, the present invention provides a fiberglass composite plate for aviation and a preparation method thereof, which has the advantage of strong environmental adaptability and solves the problem of composite plates in the prior art being sensitive to the environment and humidity.

[0006] (II) Technical solution To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a fiberglass composite plate for aviation, the plate being composed of high-performance fibers, a resin matrix and additives, and the specific raw material components and weight ratios thereof are: special alkali-free glass fiber 7%-10%; R-grade high-strength glass fiber 14%-16%; silicon carbide fiber 11%-13%; zirconium oxide fiber 20%-22%; silicone resin 6%-9%; furan resin 8%-11%; polyester imide resin 5%-6%; flame retardant 0.3%-0.4%; toughening agent 0.3%-0.5%; stabilizer 0.4%-0.7%; absorbent 1.2%-1.6%.

[0007] Preferably, the high-performance fiber is composed of special alkali-free glass fiber, R-grade high-strength glass fiber, silicon carbide fiber and zirconium oxide fiber, the resin matrix is ​​composed of silicone resin, furan resin and polyesterimide resin, and the additive is composed of flame retardant, toughening agent, stabilizer and absorber.

[0008] Preferably, the preparation steps of the special alkali-free glass fiber are: S1.1. Select raw materials: select kaolin, quartz, pyrophyllite and limestone in a ratio of 1:2:1:3 as raw materials; S1.2. Selection of auxiliary materials: epoxy resin, wetting agent, clarifier, sulfate and halide are selected as auxiliary materials; S1.3, Melting: Use a unit kiln as a combustion furnace, natural gas as fuel, and control the temperature at 1400-1500℃. Put the raw materials in the order of quartz, pyrophyllite, limestone and kaolin, and then introduce pure oxygen with a flow rate of 1000 Nm³ / h. When the temperature drops to 1000-1100℃, add clarifiers, sulfates and halides to form molten glass liquid; S1.4, wire drawing: the molten glass liquid is drawn through a platinum-rhodium alloy plate to form a continuous glass fiber strand, and the fiber strand is controlled to be 20 microns to 25 microns; S1.5, Winding: Gather multiple monofilament glass fibers into bundles and apply a sizing agent; S1.6, Dipping: Soak the glass fiber fabric in epoxy resin to make it fully saturated, and finally form special alkali-free glass fiber.

[0009] Preferably, the furan resin is prepared by homopolymerization of furfural or furfuryl alcohol or co-condensation with other monomers, and its molecular structure is: ; The molecular structure of furan resin contains a furan ring.

[0010] Preferably, a method for preparing a fiberglass composite plate for aviation is prepared according to the raw material composition and weight ratio of the above-mentioned fiberglass composite plate for aviation, and the plate preparation process is: Step 1: Pre-treat the mixed fiber: mix the special alkali-free glass fiber, R-grade high-strength glass fiber, silicon carbide fiber and zirconium oxide fiber according to the raw material ratio, and pre-treat the raw material combination; Step 2: Pre-treating the mixed resin: adding the silicone resin, furan resin and polyester imide resin into a high-speed mixer under specific conditions; Step 3: Composite sheet forming: the pretreated fibers are mixed with the pretreated mixed resin to form a prepreg material, and the prepreg material is heated and formed in a mold using a winding molding method; Step 4: Curing treatment: curing the formed composite sheet; Step 5, post-treatment 1: spraying a mixed preparation consisting of a flame retardant, a toughening agent and a stabilizer; Step 6. Post-processing 2: Spraying absorbent.

[0011] Preferably, the combination process in step one is: adding special alkali-free glass fiber and silicon carbide fiber to a fabric pretreatment furnace, setting the temperature to 500-600°C, setting the stirring speed to 800r / min for mixing, and mixing for 15-20min, and then mixing R-grade high-strength glass fiber and zirconia fiber according to the raw material ratio and adding them to the fabric pretreatment furnace, setting the temperature to 1200-1300°C, the stirring speed to 1000r / min, and the mixing time to 10-12min.

[0012] Preferably, in the resin mixing process in step 2, the silicone resin, furan resin and polyester imide resin are added into a high-speed mixer under specific conditions, and the temperature is set to 70-75° C., the stirring speed is set to 1200 r / min, and the stirring time is set to 20-24 min.

[0013] Preferably, the process of forming the composite sheet in step three is: S2.1. Dip the pretreated fiber cloth tape into the pretreated mixed resin glue solution. After dipping for 2 hours, continuously wind it on the core mold according to the line shape predetermined by the manufacturer. S2.2, put the fiber cloth tape wrapped around the core mold into an autoclave, and set the autoclave temperature to 150-155°C, and cure the resin for 20 minutes under this heating condition to form a composite sheet with a predetermined shape by the manufacturer; S2.3, demoulding after curing to obtain the final composite board.

[0014] Preferably, in the post-treatment 1 of step 5: the flame retardant, toughening agent and stabilizer are mixed at room temperature and loaded into a low-speed spray gun, the spray gun speed is set to 30-60 cm / second, and the spraying thickness is between 50 microns and 60 microns.

[0015] Preferably, in the post-processing 2 of step 6: finally, the radar absorbing agent is loaded into a low-speed spray gun, the spray gun speed is set to 30-40 cm / second, and the spraying thickness is between 20 microns and 30 microns.

[0016] Compared with the prior art, the present invention provides a fiberglass composite sheet for aviation and a preparation method thereof, which has the following beneficial effects: 1. In the preparation process of the present invention, by spraying a mixed preparation consisting of a flame retardant, a toughening agent and a stabilizer in step five, the fire resistance, toughness and stability of the composite board can be improved. By spraying an absorber in step six, the absorbing performance of the composite board can be enhanced, so that the final finished board has an advantage in resisting degradation caused by environmental factors, is suitable for long-term exposure to harsh environments, and solves the problem of composite boards being sensitive to the environment and humidity in the prior art. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 A flow chart was prepared for the present invention. DETAILED DESCRIPTION

[0018] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0019] Example 1 See also Figure 1 , a fiberglass composite sheet for aviation, the sheet is composed of high-performance fiber, resin matrix and additives, and its specific raw material composition and weight ratio are: special alkali-free glass fiber 7%-10%; R-grade high-strength glass fiber 14%-16%; silicon carbide fiber 11%-13%; zirconium oxide fiber 20%-22%; silicone resin 6%-9%; furan resin 8%-11%; polyester imide resin 5%-6%; flame retardant 0.3%-0.4%; toughening agent 0.3%-0.5%; stabilizer 0.4%-0.7%; absorbent 1.2%-1.6%; Specifically, the raw materials are: Special alkali-free glass fiber: This fiber is used in the form of fine fabric prepreg in aviation composite panels. It has corrosion resistance and electrical insulation, and also has strong resistance to interlaminar shear and tearing. R-grade high-strength glass fiber: It is a glass fiber with high mechanical strength, made of silicon-aluminum-calcium-magnesium system glass, with heat resistance and high mechanical strength, suitable for the aviation field; Silicon carbide fiber: has high temperature oxidation resistance, high hardness, high strength, high thermal stability and corrosion resistance; Zirconia fiber: has high temperature resistance and heat insulation properties and can be used in aerospace materials; Silicone resin: It has excellent high and low temperature resistance, electrical insulation, weather resistance and corrosion resistance, and can be used to prepare high-performance composite panels; Furan resin: It is a thermosetting resin with alkali resistance, solvent resistance and acid-base alternating medium resistance. It can be used as a binder for casting sand cores and can also be used to produce coatings. Polyesterimide resin: It has high temperature resistance, heat aging resistance, good mechanical properties and electrical insulation, and can be used for high-performance composite panels; Flame retardant: used to improve the flame retardancy of aviation composite panels. It can be used in plastics, rubber and fiber materials to improve the safety of composite panels. Toughening agent: can be used to improve the impact resistance and fracture toughness of aviation composite panels; Stabilizer: can be used to improve the stability of aviation composite panels to prevent degradation or performance degradation during processing or use; Radar absorber: can be used in aviation to absorb radar waves, reduce reflections, and improve the stealth performance of materials.

[0020] Specifically, the high-performance fiber is composed of special alkali-free glass fiber, R-grade high-strength glass fiber, silicon carbide fiber and zirconium oxide fiber, the resin matrix is ​​composed of silicone resin, furan resin and polyesterimide resin, and the additive is composed of flame retardant, toughening agent, stabilizer and absorber.

[0021] Specific steps for preparing special alkali-free glass fiber: S1.1. Select raw materials: select kaolin, quartz, pyrophyllite and limestone in a ratio of 1:2:1:3 as raw materials; S1.2. Selection of auxiliary materials: epoxy resin, wetting agent, clarifier, sulfate and halide are selected as auxiliary materials; S1.3, Melting: Use a unit kiln as a combustion furnace, natural gas as fuel, and control the temperature at 1400-1500℃. Put the raw materials in the order of quartz, pyrophyllite, limestone and kaolin, and then introduce pure oxygen with a flow rate of 1000 Nm³ / h. When the temperature drops to 1000-1100℃, add clarifiers, sulfates and halides to form molten glass liquid; S1.4, wire drawing: the molten glass liquid is drawn through a platinum-rhodium alloy plate to form a continuous glass fiber strand, and the fiber strand is controlled to be 20 microns to 25 microns; S1.5, Winding: Multiple monofilament glass fibers are assembled into bundles and coated with a wetting agent to prevent friction and breakage between fibers; S1.6, Dipping: Soak the glass fiber fabric in epoxy resin to make it fully saturated, and finally form special alkali-free glass fiber. This step enhances the mechanical properties and chemical corrosion resistance of the material.

[0022] Specifically, furan resin is prepared by homopolymerization of furfural or furfuryl alcohol or co-condensation with other monomers, and its molecular structure is: ; The molecular structure of furan resin contains a furan ring.

[0023] Specifically, a method for preparing a fiberglass composite plate for aviation is prepared according to the raw material composition and weight ratio of the above-mentioned fiberglass composite plate for aviation, and the plate preparation process is as follows: Step 1: Pre-treat the mixed fiber: Mix the special alkali-free glass fiber, R-grade high-strength glass fiber, silicon carbide fiber and zirconium oxide fiber according to the raw material ratio, and pre-treat the raw material combination to ensure that the combined energy efficiency is maximized, and at the same time, the raw material components are evenly distributed through stirring; Step 2: Pre-treating the mixed resin: adding the silicone resin, furan resin and polyester imide resin into a high-speed mixer under specific conditions; Step 3: Composite sheet forming: the pretreated fibers are mixed with the pretreated mixed resin to form a prepreg material, and the prepreg material is heated and formed in a mold using a winding molding method; Step 4: Curing: The formed composite sheet is cured to improve its mechanical strength and durability. This step involves high temperature curing or chemical cross-linking reaction. Step 5, post-treatment 1: spraying a mixture consisting of a flame retardant, a toughening agent and a stabilizer to improve the fire resistance, toughness and stability of the composite board; Step 6. Post-processing 2: Spray the absorber to enhance the material's absorbing properties.

[0024] Specifically, the combination process in step one is: adding special alkali-free glass fiber and silicon carbide fiber to the fabric pretreatment furnace, setting the temperature to 500-600°C, setting the stirring speed to 800r / min for mixing, and mixing for 15-20min, and then mixing R-grade high-strength glass fiber and zirconia fiber according to the raw material ratio and adding them to the fabric pretreatment furnace, setting the temperature to 1200-1300°C, the stirring speed to 1000r / min, and the mixing time to 10-12min.

[0025] Specifically, in the process of mixing the resins in step 2, the silicone resin, furan resin and polyester imide resin are added into a high-speed mixer under specific conditions, and the temperature is set to 70-75° C., the stirring speed is set to 1200 r / min, and the stirring time is set to 20-24 min.

[0026] Specifically, the process of forming the composite sheet in step 3 is as follows: S2.1. Dip the pretreated fiber cloth tape into the pretreated mixed resin glue solution. After dipping for 2 hours, continuously wind it on the core mold according to the line shape predetermined by the manufacturer. S2.2, put the fiber cloth tape wrapped around the core mold into an autoclave, and set the autoclave temperature to 150-155°C, and cure the resin for 20 minutes under this heating condition to form a composite sheet with a predetermined shape by the manufacturer; S2.3, demoulding after curing to obtain the final composite board.

[0027] Specifically, post-processing one in step five: mix the flame retardant, toughening agent and stabilizer at room temperature, and load them into a low-speed spray gun, set the spray gun speed to 30-60 cm / second, and the spray thickness to between 50 microns and 60 microns to improve the fire resistance, toughness and stability of the composite board.

[0028] Specifically, post-processing 2 in step 6: finally, the absorbent is loaded into a low-speed spray gun, the spray gun speed is set to 30-40 cm / second, and the spraying thickness is between 20 microns and 30 microns to enhance the material's absorbing performance.

[0029] Comparative Example 1 Add step 5 in Example 1 to step 3, and keep other steps unchanged.

[0030] Comparative Example 2 Add step 6 in Example 1 to step 3, and keep other steps unchanged.

[0031] A manufacturer made finished board products from Example 1 and Comparative Examples 1-2, and tested their environmental sensitivity. The test data are shown in the following table: Test items Example 1 Comparative Example 1 Comparative Example 2 Ambient humidity 85% 75% 80% aging 90% 80% 85% UV exposure 95% 85% 90% Salt spray corrosion 90% 80% 85% It can be seen from the above table that Example 1 shows higher performance indicators in all test items, especially in the aging and ultraviolet irradiation tests, which shows that Example 1, after spraying the mixed preparation composed of flame retardant, toughening agent and stabilizer in step five, can improve the fire resistance, toughness and stability of the composite board, and after spraying the absorber in step six, the absorbing performance of the composite board can be enhanced, so that the final finished board has advantages in resisting degradation caused by environmental factors and is suitable for long-term exposure to harsh environments.

[0032] Therefore, the finished board product made by the present invention has the advantage of strong environmental adaptability and solves the problem of the composite board in the prior art being sensitive to the environment and humidity.

[0033] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A fiberglass composite sheet for aviation, characterized in that: The board is composed of high-performance fibers, resin matrix and additives. Its specific raw material components and weight ratios are: special alkali-free glass fiber 7%-10%; R-grade high-strength glass fiber 14%-16%; silicon carbide fiber 11%-13%; zirconium oxide fiber 20%-22%; silicone resin 6%-9%; furan resin 8%-11%; polyester imide resin 5%-6%; flame retardant 0.3%-0.4%; toughening agent 0.3%-0.5%; stabilizer 0.4%-0.7%; absorber 1.2%-1.6%.

2. The fiberglass composite sheet for aviation use according to claim 1, characterized in that: The high-performance fiber is composed of special alkali-free glass fiber, R-grade high-strength glass fiber, silicon carbide fiber and zirconium oxide fiber, the resin matrix is ​​composed of silicone resin, furan resin and polyesterimide resin, and the additive is composed of flame retardant, toughening agent, stabilizer and absorbent.

3. The fiberglass composite sheet for aviation use according to claim 1, characterized in that: The preparation steps of the special alkali-free glass fiber are: S1.

1. Select raw materials: select kaolin, quartz, pyrophyllite and limestone in a ratio of 1:2:1:3 as raw materials; S1.

2. Selection of auxiliary materials: epoxy resin, wetting agent, clarifier, sulfate and halide are selected as auxiliary materials; S1.3, Melting: Use a unit kiln as a combustion furnace, natural gas as fuel, and control the temperature at 1400-1500℃. Put the raw materials in the order of quartz, pyrophyllite, limestone and kaolin, and then introduce pure oxygen with a flow rate of 1000 Nm³ / h. When the temperature drops to 1000-1100℃, add clarifiers, sulfates and halides to form molten glass liquid; S1.4, wire drawing: the molten glass liquid is drawn through a platinum-rhodium alloy plate to form a continuous glass fiber strand, and the fiber strand is controlled to be 20 microns to 25 microns; S1.5, Winding: Gather multiple monofilament glass fibers into bundles and apply a sizing agent; S1.6, Dipping: Soak the glass fiber fabric in epoxy resin to make it fully saturated, and finally form special alkali-free glass fiber.

4. The fiberglass composite sheet for aviation use according to claim 1, characterized in that: The furan resin is prepared by homopolymerization of furfural or furfuryl alcohol or co-condensation with other monomers, and its molecular structure is: ; The molecular structure of furan resin contains a furan ring.

5. A method for preparing a fiberglass composite sheet for aviation, characterized in that: According to the raw material composition and weight ratio of the fiberglass composite plate for aviation use described in claim 1, the plate preparation process is: Step 1: Pre-treat the mixed fiber: mix the special alkali-free glass fiber, R-grade high-strength glass fiber, silicon carbide fiber and zirconium oxide fiber according to the raw material ratio, and pre-treat the raw material combination; Step 2: Pre-treating the mixed resin: adding the silicone resin, furan resin and polyester imide resin into a high-speed mixer under specific conditions; Step 3: Composite sheet forming: the pretreated fibers are mixed with the pretreated mixed resin to form a prepreg material, and the prepreg material is heated and formed in a mold using a winding molding method; Step 4: Curing treatment: curing the formed composite sheet; Step 5, post-treatment 1: spraying a mixed preparation consisting of a flame retardant, a toughening agent and a stabilizer; Step 6. Post-processing 2: Spraying absorbent.

6. The method for preparing a fiberglass composite sheet for aviation use according to claim 5, characterized in that: The combination process in step 1 is as follows: adding the special alkali-free glass fiber and silicon carbide fiber to a fabric pretreatment furnace, setting the temperature to 500-600°C, setting the stirring speed to 800r / min for mixing, and mixing for 15-20min; then mixing the R-grade high-strength glass fiber and zirconium oxide fiber according to the raw material ratio and adding them to the fabric pretreatment furnace, setting the temperature to 1200-1300°C, setting the stirring speed to 1000r / min, and mixing for 10-12min.

7. The method for preparing a fiberglass composite sheet for aviation use according to claim 5, characterized in that: The resin mixing process in step 2 is as follows: adding the silicone resin, furan resin and polyester imide resin into a high-speed mixer under specific conditions, and setting the temperature to 70-75° C., the stirring speed to 1200 r / min, and the stirring time to 20-24 min.

8. The method for preparing a fiberglass composite sheet for aviation use according to claim 5, characterized in that: The process of forming the composite sheet in step 3 is as follows: S2.

1. Dip the pretreated fiber cloth tape into the pretreated mixed resin glue solution. After dipping for 2 hours, continuously wind it on the core mold according to the line shape predetermined by the manufacturer. S2.2, put the fiber cloth tape wrapped around the core mold into an autoclave, and set the autoclave temperature to 150-155°C, and cure the resin for 20 minutes under this heating condition to form a composite sheet with a predetermined shape by the manufacturer; S2.3, demoulding after curing to obtain the final composite board.

9. The method for preparing a fiberglass composite sheet for aviation use according to claim 5, characterized in that: Post-treatment 1 in step 5: Mix the flame retardant, toughening agent and stabilizer at room temperature and load them into a low-speed spray gun, set the spray gun speed to 30-60 cm / second, and the spray thickness to be between 50 microns and 60 microns.

10. The method for preparing a fiberglass composite sheet for aviation use according to claim 5, characterized in that: Post-processing 2 in step 6: finally, the wave absorbing agent is loaded into a low-speed spray gun, the spray gun speed is set to 30-40 cm / second, and the spraying thickness is between 20 microns and 30 microns.

Citation Information

Patent Citations

  • Production process of glass fiber reinforced plastic pultrusion profiles

    CN107009649A

  • Glass fiber reinforced composite plastic

    CN115819994A

  • Composite high-strength glass fiber reinforced plastic pultrusion profile and preparation method thereof

    CN116512642A

  • Glass fiber-reinforced composite material and production method therefor

    JP2011246595A