Composite material for wet heat preservation and solid buoyancy providing and preparation method thereof
By using silane coupling agent to modify hollow glass microbeads and modified phenolic aerogel fillers in deep-sea oil and gas pipeline materials, the problems of insufficient thermal insulation performance and low compression strength under deep-sea conditions are solved, and the excellent mechanics of composite materials are achieved and thermal insulation properties, suitable for deep-sea oil and gas pipelines and solid buoyancy applications.
Patent Information
- Application Number
- CN202411286452.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-13
AI Technical Summary
The existing wet insulation materials and solid buoyancy materials in deep-sea oil and gas pipelines have problems such as insufficient insulation performance and low compression strength under deep-sea conditions, and it is difficult to blend inorganic and organic materials, resulting in uneven material mixing.
Modified hollow glass microbeads and modified phenolic aerogel filler by using silane coupling agent. The composite material in the phenolic resin matrix is formed by agitating and defoaming machine, which improves the dispersion and interface compatibility of the filler, enhances the mechanical properties and Thermal insulation performance.
It realizes the excellent compressive strength and thermal insulation properties of composite materials, reduces material density, and improves mechanical strength and thermal insulation properties. It is suitable for deep-sea oil and gas pipelines and is suitable for moisture insulation and solid buoyancy applications, with a service depth of up to 3,000 meters.
Smart Images

Figure BDA0005043234680000061 
Figure BDA0005043234680000071
Abstract
Description
Technical Field
[0001] The invention relates to the field of organic and inorganic blended materials, and in particular to a composite material for wet heat preservation and providing solid buoyancy and a preparation method thereof. Background Art
[0002] Deep-sea oil and gas pipelines are called "the lifeline of offshore oil and gas fields" and are an important part of offshore oil and gas collection, transportation and storage systems. The basic form of the single-wall pipe insulation structure currently used at home and abroad is: steel pipe-anti-corrosion layer-insulation layer-waterproof protective layer, in which the insulation layer and the protective layer are connected with an adhesive to form the "three-proof system" of the pipeline, so that the steel pipe, anti-corrosion layer, insulation layer and protective layer are firmly combined into one, improving the anti-corrosion and thermal insulation effect of the pipeline.
[0003] Insulation materials are the core of pipeline insulation structure. Unlike traditional sandwich insulation structures, since pipeline wet insulation materials are in direct contact with seawater and bear huge hydrostatic pressure in the deep sea, their insulation performance, water absorption, tensile and compressive yield strength, high temperature adaptability, creep resistance, etc. must be considered when selecting wet insulation materials for deep-sea oil and gas pipelines. Composite foam is a material composed of hollow spherical fillers in a resin matrix, such as epoxy composite foam, polyurethane composite foam and phenolic composite foam, which have been widely used in oil pipelines in offshore operating platforms. However, the production of composite foam insulation materials for deep-sea pipelines is basically monopolized by foreign companies, such as AIS in the UK. At the same time, there are still technical problems that need to be improved when wet insulation composite foam materials are used for deep-sea pipeline insulation, the most important of which is to ensure excellent thermal insulation performance under deep-sea conditions.
[0004] In addition, in order to ensure the stable operation of oil development equipment in the deep sea, solid buoyancy materials need to be installed to provide sufficient static buoyancy. However, the solid buoyancy materials currently prepared in my country still have a lot of gaps with international advanced technologies. For example, the buoyancy materials developed in the early stage generally use polyurethane foam, epoxy resin foam or other foamed plastics. Compared with the same materials abroad, their compression strength is low, the reliability of use is poor, and the maximum working depth is only 400m.
[0005] Chinese patent CN103665768A discloses a method for preparing a high-strength solid buoyancy material. Although a coupling agent is used to modify the hollow microspheres, it does not consider the addition of other targeted fillers to further enhance the comprehensive performance of the material. Chinese patent CN109796840A discloses a reactor external insulation material, which adds silica aerogel as a filler. However, since silica aerogel is still an inorganic aerogel, it is difficult to blend inorganic and organic materials, resulting in uneven mixing of the material. Therefore, on this basis, according to the specific properties of the composite material, a specific filler is selected to solve the interface compatibility problem, and the development of a composite material for wet insulation and providing solid buoyancy is of great significance to the safe operation of my country's marine pipelines and the development of marine energy. Summary of the invention
[0006] In order to overcome the technical problems existing in the above-mentioned prior art, the present invention provides a composite material for wet insulation and providing solid buoyancy and a preparation method thereof, which has excellent compressive strength and thermal insulation performance; and the entire preparation process is simple, easy to operate, and low in cost, and is suitable for small batch sample preparation.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is:
[0008] In a first aspect, the present invention provides a composite material for wet heat preservation and providing solid buoyancy, which comprises the following preparation raw materials in parts by weight:
[0009] 100 parts of base resin, 30-60 parts of microbeads, 5-30 parts of curing agent, 0-10 parts of reinforcing filler and 0-10 parts of modified phenolic aerogel filler;
[0010] The base resin is a phenolic resin;
[0011] The microbeads are hollow glass microbeads whose surfaces are modified by coupling agents.
[0012] Preferably, the composite material for wet insulation and providing solid buoyancy comprises the following preparation raw materials in parts by weight:
[0013] 100 parts of base resin, 30-60 parts of microbeads, 5-30 parts of curing agent, 1-5 parts of reinforcing filler and 0.5-5 parts of modified phenolic aerogel filler.
[0014] Further preferably, the composite material for wet insulation and providing solid buoyancy comprises the following preparation raw materials in parts by weight:
[0015] 100 parts of base resin, 44-46 parts of microbeads, 10-12 parts of curing agent, 1-2 parts of reinforcing filler and 0.8-1.2 parts of modified phenolic aerogel filler.
[0016] Preferably, the phenolic resin has a density of 1.10-1.50 g / cm 3 , solid content is 50%-80%, and viscosity is 500-5000mPa·s / 25℃.
[0017] Preferably, the microspheres are hollow glass microspheres modified by a silane coupling agent, and the silane coupling agent is at least one of γ-aminopropyltriethoxysilane (KH550), γ-glycidyloxypropyltrimethoxysilane (KH560) and γ-methacryloxypropyltrimethoxysilane (KH570). The specific source and preparation process of the hollow glass microspheres modified by the silane coupling agent are not limited in the present invention.
[0018] Further preferably, the density of the hollow glass microspheres is 0.30-0.70 g / cm 3 , particle size is 10-200 μm, and compressive strength is 10-100 MPa. The specific source and preparation process of the hollow glass microspheres are not limited in the present invention, and hollow glass microspheres prepared by known methods or commercial hollow glass microspheres can be used.
[0019] Preferably, the curing agent includes at least one of p-toluenesulfonic acid, benzenesulfonic acid and propylene carbonate.
[0020] Preferably, the reinforcing filler is at least one of nano-silicon dioxide, glass fiber and carbon black.
[0021] Preferably, the modified phenolic aerogel filler is at least one of boron-modified phenolic resin-formaldehyde aerogel powder, benzoxazine resin-formaldehyde aerogel powder and epoxy-modified phenolic resin-formaldehyde aerogel powder.
[0022] Preferably, the preparation method of the modified phenolic aerogel filler is to mix and stir the modified phenolic resin, ethanol and urotropine (by weight) in a ratio of 1: (3-3.4): (0.2-0.4), transfer to a hydrothermal kettle at 100-160°C to react for 15-20h, and after the reaction is completed, take out, grind and sieve to obtain the modified phenolic aerogel filler. The modified phenolic resin is one of boron-modified phenolic resin, benzoxazine resin and epoxy-modified phenolic resin. The specific source of the modified phenolic resin is not limited in the present invention, and homemade or commercial modified phenolic resin can be used.
[0023] The second aspect of the present invention provides a method for preparing the composite material for wet insulation and providing solid buoyancy, comprising the following steps:
[0024] (1) After mixing the base resin and the curing agent, other preparation raw materials are added, mixed and stirred to obtain a mixture;
[0025] (2) Degassing the mixture and transferring it to a mold, curing and demoulding to obtain the composite material for wet insulation and providing solid buoyancy.
[0026] Preferably, the curing step is curing at room temperature for 10-24 hours, and then curing at 60-120° C. for 10-24 hours.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] 1. A composite material for wet insulation and providing solid buoyancy provided by the present invention uses a silane coupling agent to modify the surface of hollow glass microspheres. The "molecular bridge" of the silane coupling agent introduces it into the resin cross-linking system to improve dispersibility, while limiting the utilization of different fillers in the resin system, and improving the interface defects between the matrix resin and the microspheres, between the microspheres and the fillers, and between the matrix resin and the fillers, and synergistically enhancing the mechanical properties and thermal insulation properties of the composite material. In addition, by innovatively introducing modified phenolic aerogel powder as a filler, compared with traditional inorganic aerogel fillers, firstly, because the phenolic aerogel is an organic aerogel and the resin matrix is the same, it is convenient for the resin-filler system to be compatible, effectively reducing the internal heat conduction path and interface defects, significantly improving the effect of the filler, and making the mechanical strength and thermal insulation properties of the composite material comprehensively improved. Secondly, due to the further modification of the phenolic resin in the phenolic aerogel, the filler is given a more excellent heat-resistant and thermal insulation performance. Therefore, the composite material of the present invention has excellent mechanical strength and thermal insulation properties while having a lower density.
[0029] 2. The present invention provides a method for preparing a composite material for wet insulation and providing solid buoyancy. The mixed material is stirred and degassed by a stirring and degassing machine and an oven, and the phenolic composite foam in which each material is evenly mixed can be obtained. The whole process has low equipment requirements, simple operation, and is non-toxic and harmless. The whole preparation process is simple, easy to operate, and low in cost. In addition, the preparation method of the present invention has no strict requirements on the order of adding materials. A mixture without obvious bubbles can be obtained after stirring and degassing, which avoids the occurrence of large bubbles inside that cause the mechanical properties of the thermal insulation material to drop sharply. DETAILED DESCRIPTION
[0030] The specific embodiments of the present invention are further described below. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0031] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are commercially available unless otherwise specified.
[0032] Example 1
[0033] This embodiment provides a composite material for wet heat preservation and providing solid buoyancy, and the raw materials and weight proportions thereof are as follows:
[0034] 100 parts of phenolic resin, 45 parts of KH550 modified S38HS, 12 parts of p-toluenesulfonic acid, 1 part of glass fiber, 1 part of nano-silica, and 1 part of boron-modified phenolic resin-formaldehyde aerogel powder.
[0035] The preparation method comprises the following steps:
[0036] S1: Pre-treating hollow glass microspheres (model: S38HS; manufacturer: 3M) with γ-aminopropyltriethoxysilane (KH550), filtering and drying to obtain the KH550-modified S38HS, wherein the amount of coupling agent used is 50wt% of the mass of the glass microspheres;
[0037] S2: Boron-modified phenolic resin (appearance: yellow solid; manufacturer: Wangxin Plastic), ethanol and urotropine (by weight) were mixed and stirred in a ratio of 1:3.2:0.3, transferred to a hydrothermal kettle at 120° C. for reaction for 15 h, and after the reaction was completed, taken out, ground and finely sieved to obtain the boron-modified phenolic resin-formaldehyde aerogel powder;
[0038] S3: After mixing the phenolic resin and p-toluenesulfonic acid, add KH550-modified S38HS, glass fiber, nano-silica and boron-modified phenolic resin-formaldehyde aerogel powder, and stir for 6 minutes until the mixture is uniform;
[0039] S4: The mixture was transferred to a planetary stirring deaerator and stirred at 1000 rpm for deaeration for 10 min;
[0040] S5: After the mixture has no obvious bubbles, it is transferred to a mold, first cured at room temperature for 10 hours, then cured at 60° C. for 24 hours, and demolded to obtain the composite material.
[0041] Example 2
[0042] This embodiment provides a composite material for wet heat preservation and providing solid buoyancy, and the raw materials and weight proportions thereof are as follows:
[0043] 100 parts of phenolic resin, 45 parts of KH550 modified S38HS, 10 parts of p-toluenesulfonic acid, 1 part of glass fiber, 1 part of nano-silica, and 1 part of boron-modified phenolic resin-formaldehyde aerogel powder.
[0044] The preparation method comprises the following steps:
[0045] S1: pre-treating S38HS with γ-aminopropyltriethoxysilane, filtering and drying to obtain the KH550-modified S38HS, wherein the amount of coupling agent used is 50wt% of the mass of the glass microspheres;
[0046] S2: mixing the boron-modified phenolic resin, ethanol and urotropine (by weight) in a ratio of 1:3.2:0.3, and transferring to a hydrothermal kettle at 120° C. to react for 15 hours. After the reaction is completed, taking out, grinding and finely sieving to obtain the boron-modified phenolic resin-formaldehyde aerogel powder;
[0047] S3: After mixing the phenolic resin and p-toluenesulfonic acid, add KH550-modified S38HS, glass fiber, nano-silica and boron-modified phenolic resin-formaldehyde aerogel powder, and stir for 6 minutes until the mixture is uniform;
[0048] S4: The mixture was transferred to a planetary stirring deaerator and stirred at 1000 rpm for deaeration for 10 min;
[0049] S5: After the mixture has no obvious bubbles, it is transferred to a mold, first cured at room temperature for 10 hours, then cured at 60° C. for 24 hours, and demolded to obtain the composite material.
[0050] Example 3
[0051] This embodiment provides a composite material for wet heat preservation and providing solid buoyancy, and the raw materials and weight proportions thereof are as follows:
[0052] 100 parts of phenolic resin, 45 parts of KH550 modified S38HS, 12 parts of p-toluenesulfonic acid, 1 part of glass fiber, and 1 part of boron-modified phenolic resin-formaldehyde aerogel powder.
[0053] The preparation method comprises the following steps:
[0054] S1: pre-treating S38HS with γ-aminopropyltriethoxysilane, filtering and drying to obtain the KH550-modified S38HS, wherein the amount of coupling agent used is 50wt% of the mass of the glass microspheres;
[0055] S2: mixing the boron-modified phenolic resin, ethanol and urotropine (by weight) in a ratio of 1:3.2:0.3, and transferring to a hydrothermal kettle at 120° C. to react for 15 hours. After the reaction is completed, taking out, grinding and finely sieving to obtain the boron-modified phenolic resin-formaldehyde aerogel powder;
[0056] S3: After mixing the phenolic resin and p-toluenesulfonic acid, add KH550-modified S38HS, glass fiber and boron-modified phenolic resin-formaldehyde aerogel powder, and stir for 6 minutes until the mixture is uniform;
[0057] S4: The mixture was transferred to a planetary stirring deaerator and stirred at 1000 rpm for deaeration for 10 min;
[0058] S5: After the mixture has no obvious bubbles, it is transferred to a mold, first cured at room temperature for 10 hours, then cured at 60° C. for 24 hours, and demolded to obtain the composite material.
[0059] Example 4
[0060] This embodiment provides a composite material for wet heat preservation and providing solid buoyancy, and the raw materials and weight proportions thereof are as follows:
[0061] 100 parts of phenolic resin, 45 parts of KH550 modified S38HS, 12 parts of p-toluenesulfonic acid, 1 part of glass fiber, 1 part of silica aerogel powder (specification: particle size 15 microns; manufacturer: Zhongning Technology).
[0062] The preparation method comprises the following steps:
[0063] S1: S38HS was pretreated with γ-aminopropyltriethoxysilane, filtered and dried to obtain the KH550 modified S38HS, and the amount of coupling agent used was 50wt% of the mass of the glass microspheres;
[0064] S2: After mixing phenolic resin and p-toluenesulfonic acid, add KH550 modified S38HS, glass fiber and silica aerogel powder, and stir for 6 minutes until the mixture is uniform;
[0065] S3: The mixture was transferred to a planetary stirring deaerator and stirred at 1000 rpm for deaeration for 10 min;
[0066] S4: After the mixture has no obvious bubbles, it is transferred to a mold, first cured at room temperature for 10 hours, then cured at 60° C. for 24 hours, and demolded to obtain the composite material.
[0067] Example 5
[0068] This embodiment provides a composite material for wet heat preservation and providing solid buoyancy, and the raw materials and weight proportions thereof are as follows:
[0069] 100 parts of phenolic resin, 45 parts of KH550 modified S38HS, 12 parts of p-toluenesulfonic acid, 1 part of glass fiber, and 1 part of nano-silica.
[0070] The preparation method comprises the following steps:
[0071] S1: S38HS was pretreated with γ-aminopropyltriethoxysilane, filtered and dried to obtain the KH550 modified S38HS, and the amount of coupling agent used was 50wt% of the mass of the glass microspheres;
[0072] S2: After mixing phenolic resin and p-toluenesulfonic acid, add KH550 modified S38HS, glass fiber and nano-silica, and stir for 6 minutes until the mixture is uniform;
[0073] S3: The mixture was transferred to a planetary stirring deaerator and stirred at 1000 rpm for deaeration for 10 min;
[0074] S4: After the mixture has no obvious bubbles, it is transferred to a mold, first cured at room temperature for 24 hours, and then cured at 60° C. for 24 hours, and demolded to obtain the composite material.
[0075] Comparative Example 1
[0076] This comparative example provides a composite material for wet heat preservation and providing solid buoyancy, and the raw materials and weight proportions thereof are as follows:
[0077] 100 parts of phenolic resin, 45 parts of S38HS, 12 parts of p-toluenesulfonic acid, and 1 part of glass fiber.
[0078] The preparation method comprises the following steps:
[0079] S1: After mixing phenolic resin and p-toluenesulfonic acid, add S38HS and glass fiber and stir for 6 minutes until the mixture is uniform;
[0080] S2: The mixture was transferred to a planetary stirring deaerator and stirred at 1000 rpm for 10 min.
[0081] S3: After the mixture has no obvious bubbles, it is transferred to a mold, first cured at room temperature for 24 hours, and then cured at 60° C. for 24 hours, and demolded to obtain the composite material.
[0082] Comparative Example 2
[0083] This comparative example provides a composite material for wet heat preservation and providing solid buoyancy, and the raw materials and weight proportions thereof are as follows:
[0084] 100 parts of phenolic resin, 45 parts of S38HS, and 10 parts of p-toluenesulfonic acid.
[0085] The preparation method comprises the following steps:
[0086] S1: After mixing phenolic resin and p-toluenesulfonic acid, add S38HS and stir for 6 minutes until the mixture is uniform;
[0087] S2: The mixture was transferred to a planetary stirring deaerator and stirred at 1000 rpm for 10 min.
[0088] S3: After the mixture has no obvious bubbles, it is transferred to a mold, first cured at room temperature for 24 hours, and then cured at 60° C. for 24 hours, and demolded to obtain the composite material.
[0089] Examples 1-5 and comparative examples 1-2 were tested for performance; the density was tested according to ISO 1183 standard; the thermal insulation performance was tested according to ISO 8301 standard; the compression performance was tested according to ISO 844 standard, and the test results are shown in Table 1 below.
[0090] Table 1
[0091]
[0092]
[0093] Result analysis:
[0094] (1) From Examples 1-2, when the content of the added curing agent increases, the prepared phenolic composite foam insulation material has a lower density, a flat thermal conductivity, and better compressive strength, indicating that its curing and cross-linking degree is significantly improved. In addition, it is found that the prepared composite material has good thermal insulation performance and compressive strength while having a low density. The thermal conductivity can reach a minimum of 0.1694W / (m·K), and the compressive strength can reach a maximum of 45.303MPa, meeting the performance index requirements of the C55 phenolic composite foam produced by AIS Company of the United Kingdom, and the service water depth can reach more than 3,000 meters, indicating that it can be used in the field of wet insulation of deep-sea oil and gas pipelines and providing solid buoyancy materials.
[0095] (2) From Examples 3 and 4, compared with the case where silica aerogel filler is added, the compressive strength of the composite material with modified phenolic aerogel filler is greatly improved, and the addition of modified phenolic aerogel filler can effectively reduce the interface defects between the filler and the matrix.
[0096] (3) From Examples 1, 3, and 5, adding reinforcing fillers can effectively improve the compressive strength of the composite material, and adding modified phenolic aerogel fillers can effectively reduce the heat conduction path, significantly reduce the thermal conductivity of the composite material and improve its compressive strength. When both are added at the same time, the comprehensive performance of the composite material can reach a good balance point. Although the overall compressive strength of the material will decrease to a certain extent due to the decrease in material density, its thermal insulation performance is better than that of the composite foam with thermal insulation aerogel fillers added alone, indicating that there is a synergistic enhancement effect between the two different types of fillers.
[0097] (4) From the combination of Examples 1-5 and Comparative Examples 1-2, after surface modification of the filler, addition of phenolic aerogel filler and confined dispersion, the thermal insulation and compression properties of the composite material are significantly enhanced while the density remains relatively unchanged, which effectively demonstrates that the above preparation method can significantly enhance the thermal insulation and mechanical properties of the composite material.
[0098] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the protection scope of the present invention.
Claims
1. A composite material for wet insulation and providing solid buoyancy, characterized in that: The preparation includes the following raw materials in parts by weight: 100 parts of base resin, 30-60 parts of microbeads, 5-30 parts of curing agent, 0-10 parts of reinforcing filler and 0-10 parts of modified phenolic aerogel filler; The base resin is a phenolic resin; The microbeads are hollow glass microbeads whose surfaces are modified by coupling agents.
2. The composite material for wet insulation and providing solid buoyancy according to claim 1, characterized in that: The preparation includes the following raw materials in parts by weight: 100 parts of base resin, 30-60 parts of microbeads, 5-30 parts of curing agent, 1-5 parts of reinforcing filler and 0.5-5 parts of modified phenolic aerogel filler.
3. The composite material for wet insulation and providing solid buoyancy according to claim 1 or 2, characterized in that: The phenolic resin has a density of 1.1-1.5 g / cm 3 , solid content is 50%-80%, and viscosity is 500-5000mPa·s / 25℃.
4. The composite material for wet insulation and providing solid buoyancy according to claim 1 or 2, characterized in that: The microbeads are hollow glass microbeads modified by a silane coupling agent, and the silane coupling agent is at least one of γ-aminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane and γ-methacryloxypropyltrimethoxysilane.
5. The composite material for wet insulation and providing solid buoyancy according to claim 4, characterized in that: The density of the hollow glass microspheres is 0.3-0.7 g / cm 3 , particle size is 10-200μm, and compressive strength is 10-100MPa.
6. The composite material for wet insulation and providing solid buoyancy according to claim 1 or 2, characterized in that: The curing agent includes at least one of p-toluenesulfonic acid, benzenesulfonic acid and propylene carbonate.
7. The composite material for wet insulation and providing solid buoyancy according to claim 1 or 2, characterized in that: The reinforcing filler is at least one of nano silicon dioxide, glass fiber and carbon black.
8. The composite material for wet insulation and providing solid buoyancy according to claim 1 or 2, characterized in that: The modified phenolic aerogel filler is at least one of boron-modified phenolic resin-formaldehyde aerogel powder, benzoxazine resin-formaldehyde aerogel powder and epoxy-modified phenolic resin-formaldehyde aerogel powder.
9. A method for preparing a composite material for wet insulation and providing solid buoyancy according to any one of claims 1 to 8, characterized in that: The following steps are involved: (1) After mixing the base resin and the curing agent, other preparation raw materials are added, mixed and stirred to obtain a mixture; (2) Degassing the mixture and transferring it to a mold, curing and demoulding to obtain the composite material for wet insulation and providing solid buoyancy.
10. The method for preparing a composite material for wet insulation and providing solid buoyancy according to claim 9, characterized in that: The curing step comprises curing at room temperature for 10-24 hours, and then curing at 60-120° C. for 10-24 hours.
Citation Information
Patent Citations
Method for preparing high-strength solid buoyancy material
CN103665768A
Ultra-low density high strength buoyancy material and preparation method thereof
CN109651765A
Preparation method of normal-pressure dried phenolic aerogel composite material capable of being quickly gelatinized
CN116284971A
Heat insulation and preservation composite board and preparation method thereof
US20230264452A1