Mixing type polyurethane material for conveying belt, conveying belt covering layer and preparation method of conveying belt covering layer

By using high-temperature vulcanization to treat the mixed polyurethane material on the conveyor belt, the problem of poor wear resistance of general rubber is solved, and high-strength and ultra-wear-resistant conveyor belt materials are realized, suitable for special operation scenarios.

CN118994880APending Publication Date: 2024-11-22BEIJING UNIV OF CHEM TECH +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410614023.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-18
Filing Date
2024-05-17
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The general rubber materials of existing conveyor belts have poor wear resistance and are difficult to meet the needs of high-strength special operation scenarios.

Method used

Using mixed polyurethane material as the conveyor belt cover layer, the mixed polyurethane raw glue, lubricant, reinforcement filler, vulcanizing agent and accelerator are used to prepare high mechanical properties and ultra-wear resistance by vulcanizing the mixed polyurethane rubber, lubricant, reinforcement filler, vulcanizing agent and accelerator at high temperature. conveyor belt material.

Benefits of technology

It realizes the high strength and ultra-wear resistance of conveyor belt materials, extends the service life, and simplifies the processing technology, suitable for special operation scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004844549170000051
    Figure BDA0004844549170000051
  • Figure BDA0004844549170000091
    Figure BDA0004844549170000091
  • Figure BDA0004844549170000101
    Figure BDA0004844549170000101
Patent Text Reader

Abstract

The invention discloses a mixed polyurethane material for a conveyor belt, a conveyor belt covering layer and a preparation method of the conveyor belt covering layer. The mixing type polyurethane material for the conveying belt is prepared from the following components: mixing type polyurethane raw rubber, a lubricant, a reinforcing filler, a vulcanizing agent, an accelerant and a coupling agent. Compared with common rubber, the mixed polyurethane material can achieve high strength and super-strong wear resistance by using a small amount of filler, and the production process adopts mechanical blending, is simple to operate, can be quickly formed at a proper temperature, and is very suitable for a conveyor belt. Meanwhile, the mixing type polyurethane material is directly bonded with the canvas impregnated with isocyanate, so that the bonding force between the mixing type polyurethane material and the canvas is enhanced, and possibility is provided for applying the mixing type polyurethane material to the covering layer of the conveying belt.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of conveyor belts, and in particular to a mixed polyurethane material for conveyor belts, a conveyor belt covering layer and a preparation method thereof. Background Art

[0002] Conveyor belts, also known as transport belts, are composite products with steel wire ropes / canvas as the load-bearing skeleton and multiple layers of rubber coated on the surface. They are widely used in the mining, chemical, food and other industries. During special operations, due to the heavy weight and irregular shape of the transported objects, the rubber on the surface of the conveyor belt is inevitably scratched by the sharp surface of the transported objects. Over time, the surface of the conveyor belt is worn and damaged, resulting in a shortened service life. However, ordinary rubber such as natural rubber and EPDM rubber have limited wear resistance, making it difficult for conveyor belts to meet high-intensity special operation scenarios.

[0003] Polyurethane is composed of oligomer polyols, isocyanates and chain extenders. It is an important and widely used polymer material. It has ideal properties, such as high wear resistance, high strength, excellent shock absorption, flexibility and elasticity. The two-phase morphology of polyurethane is the result of the incompatibility of soft segments and hard segments. The morphology of polyurethane determines its physical and mechanical properties. The hard segment is composed of rigid segments bonded by hydrogen bonds formed by the reaction of diisocyanates and chain extenders, which mainly determines the modulus of polyurethane. The soft segment is composed of polyether or polyester diols, which mainly affects the elasticity of polyurethane. According to its processing method, solid polyurethane elastomers can be divided into three categories, namely, mixed polyurethane (MPU), cast polyurethane (CPU) and thermoplastic polyurethane (TPU). The hardness of CPU and TPU products is relatively high, reaching more than 70 Shore A, and mixed polyurethane is similar to ordinary rubber such as natural rubber. It can be mixed using the same processing technology, and finally high-temperature molding is used to obtain the desired products, which is more suitable for the processing and production process of conveyor belts. A great deal of research has been conducted on polyurethane composites based on cast and thermoplastic elastomers, but relatively little research has been conducted on millable polyurethane-based composites.

[0004] Therefore, there is a need for a high-strength, ultra-wear-resistant mixed polyurethane material to be used on conveyor belts to meet special operations. Summary of the invention

[0005] In order to solve the problem of poor wear resistance in general-purpose rubber materials for conveyor belts in the prior art, the present invention provides a mixed polyurethane material for conveyor belts, a conveyor belt covering layer and a preparation method thereof. Compared with general-purpose rubbers such as natural rubber and nitrile rubber, the mixed polyurethane material for conveyor belts of the present invention has higher tensile strength and superior wear resistance. The present invention uses mixed polyurethane as a matrix, mixes in relatively small amounts of reinforcing fillers, and uses a vulcanizing agent and an accelerator to perform vulcanization molding at high temperature to prepare a mixed polyurethane material with higher mechanical properties and excellent wear resistance. The present invention also provides a bonding idea, which makes it possible to use the mixed polyurethane described in the present invention in the conveyor belt covering layer.

[0006] One of the purposes of the present invention is to provide a kneadable polyurethane material for conveyor belts, which is prepared from components including kneadable polyurethane raw rubber, lubricant, reinforcing filler, vulcanizing agent, accelerator and coupling agent.

[0007] In a preferred embodiment of the present invention,

[0008] The millable polyurethane raw rubber (MPU) can be obtained from the market or by self-production. The commercially available millable polyurethane raw rubber is preferably a UR series millable polyurethane raw rubber. The UR series millable polyurethane raw rubber preferably includes at least one of UR101 and UR401 millable polyurethane raw rubbers.

[0009] Preferably,

[0010] The self-mixed polyurethane raw rubber can be prepared from components including the following raw materials:

[0011] Polyols, diisocyanates, antioxidants and chain extenders;

[0012] Each component is calculated based on 100 parts by weight of polyol.

[0013] 25-40 parts by weight of diisocyanate;

[0014] 0.3-0.5 parts by weight of antioxidant;

[0015] Chain extender 7-12 parts by weight;

[0016] The polyol is at least one of polytetrahydrofuran, polypropylene adipate, polyethylene adipate, polybutylene adipate, polycaprolactone and polycarbonate, and different polyols have different PU properties; and / or,

[0017] The antioxidant is at least one of antioxidant 1010, antioxidant 1076, and antioxidant 264, and the antioxidant can prevent oxidation of unsaturated bonds in the molecular chain; and / or,

[0018] The diisocyanate is one or a combination of two of toluene diisocyanate, 4,4'-diphenylmethane diisocyanate (MDI), 1,5-naphthalene diisocyanate, p-phenylene diisocyanate, and hexamethylene diisocyanate; and / or,

[0019] The chain extender is one or more combinations of trimethylolpropane monoallyl ether, α-glycerol allyl ether, and 1,4-butanediol.

[0020] The synthesis of the millable polyurethane raw rubber (MPU) described in the present invention can adopt the following specific technical scheme:

[0021] (1) 100 parts by weight of polyol is weighed and added to a reactor, evacuated to a vacuum and heated to 100-120° C., the stirrer is turned on and set to 250 rpm to stir and remove water until no bubbles appear in the bottle, the temperature is lowered to 60° C., 25-40 parts by weight of diisocyanate and 0.3-0.5 parts by weight of antioxidant are weighed and added to the reactor, stirred evenly, and the temperature is raised to 60-90° C. for reaction for 0.3-2 hours;

[0022] (2) Weigh 7 to 12 parts by weight of the chain extender into the reactor and stir evenly. After reacting at 60 to 90° C. for 0.3 to 2 hours, seal the reactor, place the reactor in an oven at 80 to 100° C. and cure for 6 to 24 hours. Then, take the reactor out and seal the reactor for storage.

[0023] In a preferred embodiment of the present invention,

[0024] The lubricant comprises stearic acid; and / or,

[0025] The reinforcing filler includes at least one of white carbon black and carbon black, preferably includes at least one of fumed white carbon black A200, carbon black N220, carbon black N234, and carbon black N330; the reinforcing filler can adsorb the polyurethane rubber molecular chains to form physical crosslinking points, provide rigidity for the rubber, and the polyurethane rubber molecular chains adsorbed on the surface of the filler have a certain mobility. As the external force increases, the molecular chains will be highly oriented, thereby playing a role in increasing the strength of the matrix. Compared with ordinary conveyor belt materials, the amount of filler required for the mixed polyurethane material for conveyor belts of the present invention is relatively small, and generally about 20 parts by weight can be used to prepare high-strength and super-wear-resistant products; and / or,

[0026] The vulcanizing agent may be a conventional vulcanizing agent in the art, preferably at least one of dicumyl peroxide (DCP) and sulfur; under the action of high temperature, the vulcanizing agent can cross-link the linear polyurethane rubber molecular chains through chemical bonds to form a three-dimensional network structure, thereby providing hardness, strength and elasticity to the polyurethane rubber, and changing the original physical properties and other mechanical properties of the rubber; and / or,

[0027] The accelerator includes at least one of 2-mercaptobenzothiazole (accelerator M), 2,2'-dibenzothiazole disulfide (accelerator DM), N-cyclohexyl-2-benzothiazole sulfonyl imide (accelerator CZ), N,N-dicyclohexyl-2-benzothiazole sulfonyl imide (accelerator DZ), tetramethylthiuram disulfide (accelerator TMTD), zinc dimethyldithiocarbamate (accelerator ZDMC), and zinc diethyldithiocarbamate (accelerator ZDC), preferably 2-mercaptobenzothiazole, 2,2'-dibenzothiazole disulfide, N-cyclohexyl-2-benzothiazole sulfonyl imide, N,N-dicyclohexyl-2-benzothiazole sulfonyl imide, tetramethylthiuram disulfide (accelerator TMTD), zinc dimethyldithiocarbamate (accelerator ZDMC), and zinc diethyldithiocarbamate (accelerator ZDC). At least two of methyl thiuram, zinc dimethyl dithiocarbamate, and zinc diethyl dithiocarbamate, more preferably a mixture of N-cyclohexyl-2-benzothiazole sulfonyl imide and tetramethyl thiuram disulfide, wherein the mass ratio of N-cyclohexyl-2-benzothiazole sulfonyl imide and tetramethyl thiuram disulfide is 1:(1-6), preferably 1:(1-2), for example, it can be (0.5 parts by weight: 3 parts by weight)-(2 parts by weight: 2 parts by weight); the accelerator can make the crosslinking agent more easily activated, accelerate the vulcanization rate, shorten the vulcanization time and vulcanization temperature, and at the same time improve the utilization rate of the vulcanizing agent, and increase the physical and mechanical properties of the polyurethane rubber; and / or,

[0028] The coupling agent is a conventional coupling agent in the art, preferably including at least one of bis-[γ-(triethoxysilyl)propyl]tetrasulfide (coupling agent Si-69), vinyl tri(β-methoxyethoxy)silane (coupling agent A-172), and 3-(2,3-epoxypropoxy)propyltrimethoxysilane (coupling agent KH-560); the coupling agent can improve the compatibility between the reinforcing filler and the rubber group, increase the dispersion of the reinforcing filler, and improve the reinforcing effect.

[0029] In a preferred embodiment of the present invention,

[0030] Each component is calculated based on 100 parts by weight of the mixed polyurethane raw rubber.

[0031]

[0032]

[0033] In a preferred embodiment of the present invention,

[0034] The raw materials for preparing the mixing type polyurethane material for the conveyor belt also include at least one of an active agent and an antioxidant; preferably,

[0035] The active agent includes active agent NH-2; and / or,

[0036] The antioxidant is a conventional antioxidant in the art, preferably including at least one of 2,2,4-trimethyl-1,2-dihydroquinoline polymer (antioxidant RD), N-(1,3-dimethyl)butyl-N'-phenyl-p-phenylenediamine (antioxidant 4020), β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate (antioxidant 1076), and pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate (antioxidant 1010); the antioxidant can alleviate the phenomenon of performance degradation of polyurethane rubber caused by factors such as heat and oxygen, and extend the service life of polyurethane rubber; further preferably,

[0037] Each component is calculated based on 100 parts by weight of the mixed polyurethane raw rubber.

[0038] Active agent 0 to 6.0 parts by weight; preferably 0 to 4.0 parts by weight;

[0039] Antiaging agent 0.5-1.5 parts by weight; preferably 1-1.5 parts by weight.

[0040] The lubricant, reinforcing filler, vulcanizing agent and antioxidant described in the present invention can be used in conventional amounts in the art, and the technicians can determine it according to the actual situation. In the present invention, it is preferably added in the above amounts.

[0041] The second object of the present invention is to provide a method for preparing a kneadable polyurethane material for a conveyor belt according to one of the objects of the present invention, comprising kneading components including a kneadable polyurethane raw rubber, a lubricant, a reinforcing filler, a vulcanizing agent, an accelerator, a coupling agent and optional activators and antioxidants to obtain a kneaded raw rubber, and then vulcanizing the kneaded raw rubber to obtain the kneadable polyurethane material for a conveyor belt.

[0042] In a preferred embodiment of the present invention,

[0043] The millable polyurethane rubber is first dehydrated before milling. Preferably, the dehydration comprises the steps of thinning the millable polyurethane rubber through rollers on an open mill and then dehydrating the rubber under vacuum.

[0044] In a preferred embodiment of the present invention,

[0045] The mixed raw rubber further includes a step of being left standing for more than 7 days after vulcanization.

[0046] The present invention can adopt the following specific technical solutions:

[0047] (1) The mixed polyurethane is thinned by rollers on an open mill, cut into suitable sizes, and placed in a vacuum oven for drying. Water is removed at a temperature of 60 to 80°C and vacuum (preferably under a negative pressure of -0.1 MPa) for 5 to 24 hours. Due to its strong polarity, polyurethane will slowly absorb moisture from the air during storage, which will affect the performance of the system. The hardness of the sample is relatively soft, and the mechanical properties and wear resistance are relatively poor.

[0048] (2) The mixed polyurethane raw rubber is plasticized on a double-roll open mill at 40-60°C for 3-5 minutes, and then the lubricant, coupling agent, optional antioxidant, and reinforcing filler are added and blended uniformly. Due to the addition of coupling agent, it is necessary to mix in an internal mixer at 140-160°C and 20-40r / min for 2-10 minutes before discharging, and preferably sealed and placed for more than 8 hours. Finally, a vulcanizing agent, an accelerator, and an optional activator are added on a double-roll open mill, blended uniformly, and the sheet is discharged and sealed and placed for 24 hours to obtain a mixed raw rubber.

[0049] (3) Place the mixed rubber into the corresponding mold (pre-sprayed with release agent) and vulcanize it in a flat vulcanizer at a temperature of 150-160°C and a pressure of 10-20 MPa for 10-40 minutes (the specific time is measured by the rotorless vulcanizer). 90 +2-3min as the standard) vulcanization molding, and storage at room temperature for more than 7 days to obtain a mixed polyurethane elastomer material. Storage for more than one week is to stabilize the internal phase of the polyurethane, which can further improve the performance of the mixed polyurethane.

[0050] The kneadable polyurethane material for conveyor belts of the present invention uses kneadable polyurethane raw rubber as base rubber, adds reinforcing filler into the raw rubber for kneading, and simultaneously mixes peroxide or sulfur for vulcanization, and performs compression vulcanization at high temperature to prepare a kneadable polyurethane elastomer material. The prepared polyurethane elastomer material has excellent mechanical properties, high strength, and excellent wear resistance.

[0051] The third object of the present invention is to provide a conveyor belt covering layer, including the mixed polyurethane material for conveyor belt according to one of the objects of the present invention or the mixed polyurethane material for conveyor belt obtained by the preparation method of the second object of the present invention; preferably, the conveyor belt covering layer has a laminated structure, including at least two layers of mixed polyurethane material for conveyor belt and at least one layer of nylon canvas, and the outer layers of the conveyor belt covering layer are all mixed polyurethane material layers for conveyor belt.

[0052] In a preferred embodiment of the present invention,

[0053] The nylon canvas is a nylon canvas impregnated with isocyanate, and the impregnation includes: immersing the nylon canvas in a phenol-blocked isocyanate pre-impregnation solution, then taking it out for rolling, drying, high-temperature curing, and then using standard RFL dipping treatment; preferably, the impregnation specifically includes: immersing the canvas in a phenol-blocked MDI pre-impregnation solution for 2 to 5 minutes, then taking it out for rolling for 1 to 5 minutes, spreading it flat in a high-temperature oven, drying it at 120 to 150°C for 10 to 15 minutes, and then subjecting it to a high-temperature curing treatment at 220 to 240°C for 3 to 10 minutes. Then use standard RFL dipping treatment to obtain a modified canvas. There is no special requirement for the process of standard RFL dipping treatment in the present invention, and any existing dipping treatment process in the art can be used.

[0054] The fourth object of the present invention is to provide a method for preparing a conveyor belt covering layer according to the third object of the present invention, comprising the step of bonding a nylon canvas layer to the mixed polyurethane material layer for the conveyor belt.

[0055] In a preferred embodiment of the present invention,

[0056] The method comprises:

[0057] The step of laminating the nylon canvas layer and the mixed raw rubber layer of the mixed polyurethane material for the conveyor belt before vulcanization and then performing mold vulcanization.

[0058] The conveyor belt covering layer of the present invention can be prepared by the following specific scheme:

[0059] Cut the nylon canvas into samples of a certain shape, and stick the same size of 0.1-5mm (preferably about 0.7mm) thick raw rubber to the upper and lower layers of the two layers of canvas and between the two layers of canvas. Finally, attach two pieces of 1-20mm (preferably about 8mm) thick raw rubber to the upper and lower sides of the sample, and put the whole into a mold to close the mold. Put it in a flat vulcanizer at 150-160℃ and 10-20MPa pressure for 10-40min (the specific time is measured by the rotorless vulcanizer t 90+ The adhesion performance test can be carried out after being placed at room temperature for 7 days.

[0060] Compared with the prior art, the present invention has the following beneficial effects:

[0061] The present invention utilizes the advantages of micro-phase separation of polyurethane soft segment and hard segment, good wear resistance and large adjustable performance range, and the obtained mixed polyurethane elastomer not only has excellent mechanical properties, but also can effectively solve the problem of limited wear resistance of common rubbers such as natural rubber and styrene-butadiene rubber. Compared with common rubber, mixed polyurethane can use less amount of filler, so as to achieve higher strength and super wear resistance, and the present invention adopts mechanical blending, is simple to operate, and can be quickly formed at a suitable temperature, which is very suitable for the production process of conveyor belts. At the same time, the present invention adopts mixed polyurethane to directly bond with canvas impregnated with isocyanate, which enhances the bonding force between canvas and the mixed polyurethane elastomer, and provides the possibility for the mixed polyurethane material described in the present invention to be applied to the conveyor belt cover layer. DETAILED DESCRIPTION

[0062] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.

[0063] The raw material information used in the embodiments and comparative examples is as follows:

[0064] The UR series of mixed polyurethane raw rubber grades are UR101 and UR401, and both raw rubbers and the active agent NH-2 are purchased from Guangdong Huagong Fosu New Materials Co., Ltd.;

[0065] The other raw materials mentioned are all common commercially available products.

[0066] Method for determining tensile stress-strain properties of samples: GB / T 528-2009 Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber.

[0067] Sample hardness determination method: GB / T 531-1999 Rubber pocket hardness tester indentation hardness test method.

[0068] Determination method of sample wear resistance: GB / T 9867-2008 Determination of wear resistance of vulcanized rubber or thermoplastic rubber (rotating roller abrasion machine method).

[0069] Determination method of sample peel strength: GB / T 6759-2013 Determination method of interlayer adhesion strength of conveyor belts.

[0070] Example 1

[0071]

[0072] The preparation process of mixed polyurethane conveyor belt materials is as follows:

[0073] (1) On an open mill, UR101 mixed polyurethane raw rubber was thinned by a roller, cut into appropriate sizes, placed in a vacuum oven for drying, and vacuumed to remove water at 70°C for 12 hours;

[0074] (2) 100 parts by weight of the UR101 mixed polyurethane raw rubber treated in step (1) was plasticized on a double-roll open mill at 50° C. for 4 min, followed by adding 0.5 parts by weight of stearic acid SA, 1.5 parts by weight of antioxidant 1076, 20 parts by weight of white carbon black A200, and 1 part by weight of coupling agent Si-69 to mix evenly, placing the mixed rubber in an internal mixer at 155° C. for mixing for 5 minutes, and then placing the mixed rubber in an open mill at 50° C. again, adding 2.0 parts by weight of accelerator TMTD, 2.0 parts by weight of accelerator CZ, 1.0 parts by weight of active agent NH-2, and 2.0 parts by weight of sulfur to mix evenly, discharging the sheet, sealing it, and placing it for 24 hours to obtain the mixed raw rubber.

[0075] (3) The mixed raw rubber was vulcanized in a flat vulcanizer at a temperature of 155° C. and a pressure of 20 MPa for 22 min, and the sample was left for 7 days to obtain a mixed polyurethane material for a conveyor belt.

[0076] Preparation of conveyor belt covering layer: The mixed raw rubber prepared according to the formula and process in Example 1 is bonded with the canvas impregnated with isocyanate. The specific process is as follows:

[0077] (1) Preparation of phenol-terminated MDI: 13.6 g of MDI was added to 100 ml of anhydrous butyl acetate solvent at 50° C., and a butyl acetate solution of phenol and a catalyst dibutyltin dilaurate (prepared by dissolving 10 g of phenol and 0.01 g of dibutyltin dilaurate in 100 ml of butyl acetate) was continuously added dropwise under a nitrogen atmosphere for 15 minutes. After reacting for 2 hours, butyl acetate was evaporated to obtain phenol-terminated MDI. Nylon 66 canvas was soaked in a pre-impregnation solution containing phenol-terminated MDI (which consisted of 100 parts by mass of deionized water, 7.59 parts by mass of phenol-terminated MDI and 1.48 parts by mass of epoxy resin EP137) for 4 minutes, then taken out and pressed for 2 minutes, spread flat in a high-temperature oven, dried at 120° C. for 15 minutes, and then subjected to a high-temperature curing treatment at 230° C. for 6 minutes. Then, it was treated with a self-made standard RFL dipping solution, the RFL solution composition was 100 parts by weight of deionized water, 12.26 parts by weight of resorcinol, 7.30 parts by weight of formaldehyde solution (37%), 1.84 parts by weight of sodium hydroxide solution (10%), 6.13 parts by weight of ammonia water and 99.74 parts by weight of VP latex solution (40%). The dipping process was to immerse the pre-impregnated canvas in the RFL dipping solution for 2 minutes, then take it out, calender for 1 minute, spread it in a 150°C high-temperature oven and dry it for 15 minutes, then transfer it to a 220°C oven for curing for 6 minutes to obtain the modified canvas, which was placed in a closed desiccator and stored away from light for later use.

[0078] (2) Cut the modified canvas into samples of 200 cm × 110 cm in size, and attach 0.7 mm thick raw rubber of the same size to the upper and lower layers of the two layers of canvas and between the two layers of canvas. Finally, attach two pieces of 8 mm thick raw rubber to the upper and lower sides of the sample, and place the whole in a mold. Vulcanize it in a flat vulcanizer at 155 ° C and 20 MPa for 30 minutes to obtain the conveyor belt cover layer. After standing at room temperature for 7 days, the peel strength test is performed.

[0079] Example 2

[0080]

[0081] The preparation process of mixed polyurethane conveyor belt materials is as follows:

[0082] (1) On an open mill, UR101 mixed polyurethane raw rubber was thinned by a roller, cut into appropriate sizes, placed in a vacuum oven for drying, and vacuumed to remove water at 70°C for 12 hours;

[0083] (2) 100 parts by weight of the UR101 mixed polyurethane raw rubber treated in step (1) was plasticized on a double-roller mill at 50° C. for 4 min, followed by adding 0.5 parts by weight of stearic acid SA, 1.5 parts by weight of antioxidant 1076, 20 parts by weight of white carbon black A200, and 1 part by weight of coupling agent Si-69 to mix evenly, and the mixed rubber was placed in an internal mixer at 155° C. for mixing for 5 minutes, and then the mixed rubber was placed in an open mixer at 50° C. again, and 4.0 parts by weight of accelerator TMTD, 1.0 parts by weight of active agent NH-2, and 2.0 parts by weight of sulfur were added to mix evenly, and the mixed rubber was sheeted and sealed for 24 hours to obtain a mixed raw rubber.

[0084] (3) The mixed raw rubber was vulcanized in a flat vulcanizer at a temperature of 155° C. and a pressure of 20 MPa for 22 min, and the sample was left for 7 days to obtain a mixed polyurethane material for a conveyor belt.

[0085] The preparation process of the conveyor belt covering layer is the same as that of Example 1 except for the formula of the mixed polyurethane material.

[0086] Example 3

[0087]

[0088] The preparation process of mixed polyurethane conveyor belt materials is as follows:

[0089] (1) On an open mill, UR101 mixed polyurethane raw rubber was thinned by a roller, cut into appropriate sizes, placed in a vacuum oven for drying, and vacuumed to remove water at 70°C for 12 hours;

[0090] (2) 100 parts by weight of the UR101 mixed polyurethane raw rubber treated in step (1) was plasticized on a double-roll open mill at 50° C. for 4 min, followed by adding 0.5 parts by weight of stearic acid SA, 1.5 parts by weight of antioxidant 1076, 20 parts by weight of white carbon black A200, and 1 part by weight of coupling agent Si-69 to mix uniformly, and the mixed rubber was placed in an internal mixer at 155° C. for mixing for 5 minutes, and then the mixed rubber was placed in an open mill at 50° C. again, and 4.0 parts by weight of accelerator CZ, 1.0 parts by weight of active agent NH-2, and 2.0 parts by weight of sulfur were added to mix uniformly, and the mixed rubber was sheeted and sealed for 24 hours to obtain a mixed raw rubber.

[0091] (3) The mixed raw rubber was vulcanized in a flat vulcanizer at a temperature of 155° C. and a pressure of 20 MPa for 22 min, and the sample was left for 7 days to obtain a mixed polyurethane material for a conveyor belt.

[0092] The preparation process of the conveyor belt covering layer is the same as that of Example 1 except for the formula of the mixed polyurethane material.

[0093] Example 4

[0094]

[0095] The preparation process of mixed polyurethane conveyor belt materials is as follows:

[0096] (1) On an open mill, UR101 mixed polyurethane raw rubber was thinned by a roller, cut into appropriate sizes, placed in a vacuum oven for drying, and vacuumed to remove water at 70°C for 12 hours;

[0097] (2) 100 parts by weight of the UR101 mixed polyurethane raw rubber treated in step (1) was plasticized on a double-roll open mill at 50° C. for 4 min, followed by adding 0.5 parts by weight of stearic acid SA, 1.5 parts by weight of antioxidant 1076, 20 parts by weight of white carbon black A200, and 1 part by weight of coupling agent Si-69 to mix evenly, placing the mixed rubber in an internal mixer at 155° C. for mixing for 5 minutes, and then placing the mixed rubber in an open mill at 50° C. again, adding 2.0 parts by weight of accelerator TMTD, 3.0 parts by weight of accelerator CZ, 1.0 parts by weight of active agent NH-2, and 2.0 parts by weight of sulfur to mix evenly, discharging the sheet, sealing it, and placing it for 24 hours to obtain the mixed raw rubber.

[0098] (3) The mixed raw rubber was vulcanized in a flat vulcanizer at a temperature of 155° C. and a pressure of 20 MPa for 22 min, and the sample was left for 7 days to obtain a mixed polyurethane material for a conveyor belt.

[0099] The preparation process of the conveyor belt covering layer is the same as that of Example 1 except for the formula of the mixed polyurethane material.

[0100] Example 5

[0101]

[0102] The preparation process of mixed polyurethane conveyor belt materials is as follows:

[0103] (1) On an open mill, UR101 mixed polyurethane raw rubber was thinned by a roller, cut into appropriate sizes, placed in a vacuum oven for drying, and vacuumed to remove water at 70°C for 12 hours;

[0104] (2) 100 parts by weight of the UR101 mixed polyurethane raw rubber treated in step (1) was plasticized on a double-roll open mill at 50° C. for 4 min, and then 0.5 parts by weight of stearic acid SA, 1.0 parts by weight of antioxidant 1076, 20 parts by weight of white carbon black A200, and 1 part by weight of coupling agent Si-69 were added and blended uniformly. The mixed rubber was placed in an internal mixer at 155° C. for 5 minutes, and then the mixed rubber was placed in an open mill at 50° C. again, and 0.2 parts by weight of accelerator TMTD and 0.5 parts by weight of DCP were added and blended uniformly. Sheets were produced and sealed and placed for 24 hours to obtain mixed raw rubber.

[0105] (3) The mixed raw rubber was vulcanized in a flat vulcanizer at a temperature of 155° C. and a pressure of 20 MPa for 22 min, and the sample was left for 7 days to obtain a mixed polyurethane material for a conveyor belt.

[0106] The preparation process of the conveyor belt covering layer is the same as that of Example 1 except for the formula of the mixed polyurethane material.

[0107] Comparative Example 1

[0108] According to the formula of Example 1, except that the UR101 mixed polyurethane raw rubber was not dried to remove water, other steps were the same as Example 1 to prepare a mixed polyurethane sample. After mechanical properties and wear resistance tests, the test results of the sample properties are shown in Table 1.

[0109] Comparative Example 2

[0110] According to the formula of Example 1, the only difference from Example 1 is that the mixed polyurethane material after mixing and vulcanization is not stored for more than 7 days, but only stored at room temperature for 1 day. The prepared mixed polyurethane sample is tested for mechanical properties and wear resistance. The test results of the sample performance are shown in Table 1.

[0111] Comparative Example 3

[0112]

[0113] The preparation process is as follows:

[0114] (1) 100 parts by weight of natural rubber NR was plasticized on a double-roll mill at 40° C. for 3 min, and then 2.0 parts by weight of stearic acid SA, 3.0 parts by weight of zinc oxide, 10761.5 parts by weight of antioxidant, and 23450 parts by weight of carbon black N2 were added and blended uniformly. Finally, 1.0 parts by weight of accelerator NS and 1.75 parts by weight of sulfur were added and blended uniformly, and the sheet was produced and sealed and placed for 24 hours.

[0115] (2) The mixed raw rubber is vulcanized in a flat plate vulcanizer at a temperature of 125° C. and a pressure of 20 MPa for 25 min to obtain a natural rubber vulcanizate.

[0116] The mechanical properties of the mixed polyurethane materials for conveyor belts obtained in Examples 1 to 5 and the vulcanized rubbers obtained in Comparative Examples 1 to 3 were tested. The results are shown in Table 1.

[0117] Table 1 Mechanical properties and wear resistance of samples of embodiments and comparative examples

[0118]

[0119] The peel strength of the transmission belt materials of Examples 1-5 was tested, and the results are shown in Table 2.

[0120] Table 2 Peel strength of Examples 1-5

[0121] Sample name <![CDATA[Average peel strength / N·mm -1 > Example 1 8.2 Example 2 7.6 Example 3 6.7 Example 4 6.5 Example 5 7.3

[0122] Comparing the mechanical properties and wear resistance of Example 1 with those of Examples 2 to 3, it can be seen that the compounded accelerator TMTD and accelerator CZ can achieve a better vulcanization effect, and the obtained polyurethane elastomer has better strength and wear resistance. Comparing the mechanical properties and wear resistance of Example 1 with those of Example 4, it can be seen that too much accelerator cannot better promote the vulcanization of vulcanized rubber, but will have a certain inhibitory effect, causing the strength and wear resistance of the obtained polyurethane elastomer to decrease. Therefore, the amount of accelerator needs to be controlled at an appropriate ratio, preferably 0.01 to 4.0 parts by weight in the present invention.

[0123] Comparing the mechanical properties and wear resistance of Example 1 with those of Comparative Example 1, drying and removing water from the mixed polyurethane raw rubber can improve the hardness, mechanical properties and wear resistance of the product; comparing the mechanical properties and wear resistance of Example 1 with those of Comparative Example 2, the wear resistance of the vulcanized mixed polyurethane material is significantly improved after being stored for 7 days and the internal structure is stabilized.

[0124] Comparing the mechanical properties and wear resistance of Examples 1 to 5 with those of Comparative Example 3, it can be seen that the hardness of the mixed polyurethane material can be controlled within the range of 60 to 70 Shore A, the tensile strength can reach more than 30 MPa, and the DIN wear volume can preferably reach 40 mm 3 Compared with ordinary rubber, the compounded polyurethane elastomer material uses relatively less filler, has higher mechanical properties, and has a significantly lower wear volume than ordinary rubber, and has the characteristics of high strength and super wear resistance.

[0125] From Table 2, it can be seen that the mixed polyurethane materials of Examples 1 to 5 have good adhesion to the isocyanate-impregnated nylon 66 canvas, and the average peel strength is 6N·mm -1 As described above, this idea provides the possibility for the mixed polyurethane material of the present invention to be applied to the conveyor belt cover layer.

[0126] The above embodiments have described the specific contents of the present invention in detail, but the present invention is not limited to the embodiments. Those skilled in the art can make various equivalent substitutions, such as changing the types and amounts of reinforcing fillers, the types and amounts of vulcanizers and other small materials, and using different feeding sequences / implementation processes / product molding processes to process the high-strength, super-wear-resistant mixed polyurethane elastomer described in the present invention. These equivalent modifications or replacements of the processing processes before and after processing and their details also fall within the scope of protection required by this application. At the same time, the application idea (bonding) of the mixed polyurethane in the conveyor belt cover also falls within the scope of protection required by this application.

Claims

1. A kneadable polyurethane material for a conveyor belt, which is prepared from components including kneadable polyurethane raw rubber, a lubricant, a reinforcing filler, a vulcanizing agent, an accelerator and a coupling agent.

2. The millable polyurethane material for conveyor belt according to claim 1, Features: The kneadable polyurethane raw rubber is a UR series kneadable polyurethane raw rubber and / or a kneadable polyurethane raw rubber prepared from components including the following raw materials: polyol, diisocyanate, antioxidant and chain extender; and / or, The lubricant comprises stearic acid; and / or, The reinforcing filler comprises at least one of white carbon black and carbon black, preferably comprises at least one of fumed white carbon black A200, carbon black N220, carbon black N234 and carbon black N330; and / or, The vulcanizing agent includes at least one of dicumyl peroxide and sulfur; and / or, The accelerator includes at least one of 2-mercaptobenzothiazole, 2,2'-dibenzothiazole disulfide, N-cyclohexyl-2-benzothiazole sulfonyl imide, N,N-dicyclohexyl-2-benzothiazole sulfonyl imide, tetramethylthiuram disulfide, zinc dimethyldithiocarbamate, and zinc diethyldithiocarbamate, preferably 2-mercaptobenzothiazole, 2,2'-dibenzothiazole disulfide, N-cyclohexyl-2-benzothiazole sulfonyl imide. At least two of imine, N,N-dicyclohexyl-2-benzothiazolesulfonyl imide, tetramethylthiuram disulfide, zinc dimethyldithiocarbamate, and zinc diethyldithiocarbamate, more preferably a mixture of N-cyclohexyl-2-benzothiazolesulfonyl imide and tetramethylthiuram disulfide, wherein the mass ratio of the mixture of N-cyclohexyl-2-benzothiazolesulfonyl imide and tetramethylthiuram disulfide is 1:(1-6); and / or, The coupling agent includes at least one of bis-[γ-(triethoxysilyl)propyl]tetrasulfide, vinyl tri(β-methoxyethoxy)silane, and 3-(2,3-epoxypropoxy)propyltrimethoxysilane.

3. The millable polyurethane material for conveyor belt according to claim 1 or 2, Features: Each component is calculated based on 100 parts by weight of the mixed polyurethane raw rubber. Lubricant 0.1 to 1 parts by weight; preferably 0.3 to 0.5 parts by weight; 10 to 40 parts by weight of reinforcing filler; preferably 10 to 30 parts by weight; 0.1 to 2.5 parts by weight of vulcanizing agent; preferably 0.5 to 2 parts by weight; Accelerator 0-6.0 parts by weight; preferably 0.01-4.0 parts by weight; The coupling agent is 0.1 to 5 parts by weight, preferably 0.1 to 2 parts by weight.

4. The millable polyurethane material for conveyor belt according to claim 1, Features: The raw materials for preparing the mixing type polyurethane material for the conveyor belt also include at least one of an active agent and an antioxidant; preferably, The active agent includes active agent NH-2; and / or, The antioxidant includes at least one of 2,2,4-trimethyl-1,2-dihydroquinoline polymer, N-(1,3-dimethyl)butyl-N'-phenyl-p-phenylenediamine, β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid n-octadecyl alcohol ester, and tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid] pentaerythritol ester.

5. A method for preparing a kneadable polyurethane material for a conveyor belt as described in any one of claims 1 to 4, comprising kneading components including kneadable polyurethane raw rubber, a lubricant, a reinforcing filler, a vulcanizing agent, an accelerator, a coupling agent and optional activators and antioxidants to obtain a kneaded raw rubber, and then vulcanizing the kneaded raw rubber to obtain the kneadable polyurethane material for a conveyor belt.

6. The preparation method according to claim 5, Features: The millable polyurethane rubber is first dehydrated before milling. Preferably, the dehydration comprises the steps of thinning the millable polyurethane rubber through rollers on an open mill and then dehydrating the rubber under vacuum.

7. A conveyor belt covering layer, comprising the mixed polyurethane material for conveyor belts according to any one of claims 1 to 4 or the mixed polyurethane material for conveyor belts obtained by the preparation method according to any one of claims 5 to 6; preferably, the conveyor belt covering layer has a laminated structure, including at least two layers of mixed polyurethane material for conveyor belts and at least one layer of nylon canvas, and the outer layers of the conveyor belt covering layer are all mixed polyurethane material layers for conveyor belts.

8. The conveyor belt cover according to claim 7, Features: The nylon canvas is nylon canvas impregnated with isocyanate, and the impregnation includes: immersing the nylon canvas in a phenol-blocked isocyanate pre-impregnation liquid, then taking it out for rolling, drying, high-temperature curing, and then using standard RFL dipping treatment.

9. A method for preparing a conveyor belt covering layer as claimed in claim 7 or 8, comprising the step of bonding a nylon canvas layer to the mixed polyurethane material layer for the conveyor belt.

10. The preparation method according to claim 9, Features The method comprises: The step of laminating the nylon canvas layer and the mixed raw rubber layer of the mixed polyurethane material for the conveyor belt before vulcanization and then performing mold vulcanization.

Citation Information

Patent Citations

  • Light and high-strength rubber conveyor belt and preparation method thereof

    CN102530469A

  • Preparation method for basalt fiber conveying belt

    CN104692027A

  • Hydrolysis-resistant polyurethane rubber and preparation method thereof

    CN107868223A

  • High-temperature-resistant polyether polyurethane rubber and preparation method thereof

    CN108102343A

  • Blend vulcanized rubber and preparation method thereof

    CN109054343A