High-strength carbon fiber skin material, preparation method and application of high-strength carbon fiber skin material in fin structural component

By using surface-modified aluminum-doped silicon carbide nanowires and polyamic acid mixed solution in carbon fiber skin material, the problem of insufficient material strength and thermal physical properties is solved, and the problem of achieving the goal of achieving It has high strength, high toughness and excellent thermal management performance, and is suitable for high-end equipment manufacturing and aerospace fields.

CN118994903APending Publication Date: 2024-11-22湖南弘辉科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411197358.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing carbon fiber skin materials have shortcomings in strength and thermal physical properties, making it difficult to meet the demanding aerospace environment needs, especially in high Mach number flight and high temperature conditions.

Method used

The semiconglomerate interface and bamboo nodes are constructed by using surface-modified aluminum-doped silicon carbide nanowires and carbon fiber composites. morphology, combined with the self-healing properties of the mixed solution of polyamic acid, improve the mechanical and thermal physical properties of the material.

Benefits of technology

It significantly improves the strength, toughness and thermal conductivity of carbon fiber composite materials, reduces the coefficient of thermal expansion, extends service life, and enhances fatigue resistance, and is suitable for high-end equipment manufacturing and aerospace fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994903A_ABST
    Figure CN118994903A_ABST
Patent Text Reader

Abstract

The invention relates to the field of carbon fiber composite materials, in particular to a high-strength carbon fiber skin material, a preparation method and application of the high-strength carbon fiber skin material in a fin structural component, and the high-strength carbon fiber skin material is prepared from the following raw materials: a surface modified aluminum doped silicon carbide nanowire / carbon fiber composite preform and a polyamide acid mixed solution; the surface modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform is prepared by carrying out PSS-[3-(2-aminoethyl) amino] propyl-substituted heptaisobutyl surface modification on the aluminum-doped silicon carbide nanowire / carbon fiber composite preform; the aluminum-doped silicon carbide nanowire / carbon fiber composite preform comprises a carbon fiber preform and aluminum-doped silicon carbide nanowires loaded on the surface of the carbon fiber preform; according to the invention, the problem of insufficient mechanical and thermal physical properties of a skin material is solved, and the durability, damage resistance and overall performance of a fin structural member are remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of carbon fiber composite materials, and in particular to a high-strength carbon fiber skin material, a preparation method and application in wing structure parts. Background Art

[0002] Carbon fiber composite materials are widely used in the aerospace field due to their excellent properties such as high specific strength and high specific modulus. In particular, in key structural parts of high-speed aircraft such as aerospace, carbon fiber composite materials are often used as skin materials, which undertake important functions such as maintaining shape, transferring loads, and resisting aerodynamic heat. With the continuous development of flight technology, higher requirements are placed on the strength performance of skin materials. On the one hand, higher strength means better structural efficiency, and a larger warhead load ratio can be obtained at the same take-off mass, thereby significantly improving the damage efficiency of the aircraft. On the other hand, the high strength of the skin material is also the key guarantee for maintaining structural integrity in harsh service environments. Extreme conditions include aerodynamic heat during high Mach number flight and inertial loads during high overload maneuvers. Only when the skin material has sufficient strength can structural damage be avoided and the reliability of the aircraft be ultimately ensured. Therefore, the development of high-strength carbon fiber skin materials is of great significance to promoting the advancement of aircraft technology. Related fields urgently need to carry out systematic and in-depth research work in order to obtain a new generation of skin materials with significantly improved strength performance.

[0003] At present, although carbon fiber skin materials have made a lot of progress, there are still some shortcomings. (1) The high strength still needs to be further improved to meet the requirements of more stringent use environments. For example, the Chinese patent with publication number CN108749229A discloses a lower skin layer material of carbon fiber cloth reinforced resin material. However, due to the natural physical and chemical property differences between carbon fiber and resin matrix, the interface bonding strength between carbon fiber and resin matrix needs to be improved. (2) The thermal physical properties are poor. The realization and maintenance of low expansion coefficient and high thermal conductivity is still one of the technical difficulties. Carbon fiber skin materials need to achieve low expansion coefficient and high thermal conductivity during service. This is because the skin material faces a severe aerodynamic heating environment and the temperature rises sharply. If the expansion coefficient of the material is too large, the deformation caused by thermal expansion will change the shape of the aircraft, destroy the aerodynamic shape, increase air resistance, and reduce the flight speed and range. At the same time, thermal deformation will also cause stress concentration, resulting in skin cracking, delamination and other damage. In severe cases, it may cause structural damage, affecting the structural integrity and reliability of the aircraft. During high-speed flight, the aircraft skin material will absorb a large amount of heat. High thermal conductivity ensures that the heat can be quickly transferred to the interior of the aircraft or other heat dissipation systems, thereby maintaining the temperature of the skin material stable and preventing performance degradation or damage due to overheating. Therefore, low expansion coefficient and high thermal conductivity are essential to maintaining the aerodynamic shape and structural integrity of the aircraft. Summary of the invention

[0004] (1) Technical issues solved

[0005] The purpose of the present invention is to provide a high-strength carbon fiber skin material, a preparation method and application in wing structure parts, so as to solve the problem of insufficient strength and thermal physical properties of current carbon fiber skin materials.

[0006] (2) Technical solution

[0007] In order to achieve the above object, the present invention provides the following technical solutions:

[0008] A high-strength carbon fiber skin material is prepared from the following raw materials in parts by weight: 30 to 55 parts of a surface-modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform and 40 to 70 parts of a polyamic acid mixed solution;

[0009] The surface-modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform is prepared by surface-modifying the aluminum-doped silicon carbide nanowire / carbon fiber composite preform with PSS-[3-(2-aminoethyl)amino]propyl-substituted heptaisobutyl; the aluminum-doped silicon carbide nanowire / carbon fiber composite preform comprises a carbon fiber preform and an aluminum-doped silicon carbide nanowire loaded on the surface of the carbon fiber preform.

[0010] In the aluminum-doped silicon carbide nanowire / carbon fiber composite preform of the present invention, firstly, the high-strength characteristics of the silicon carbide nanowire itself also directly contribute to the improvement of the overall strength of the composite material. Secondly, as a typical low expansion coefficient material, the nanoscale introduction of silicon carbide can significantly affect the thermal expansion behavior of the composite material. The uniform distribution of silicon carbide nanowires on the surface of carbon fiber forms an effective thermal stress buffer layer, which can evenly disperse and alleviate the thermal stress concentration caused by temperature changes. In addition, the interaction between silicon carbide nanowires and the polyimide resin matrix also promotes the uniform distribution of thermal stress inside the composite material, thereby further reducing the overall thermal expansion coefficient. Finally, silicon carbide nanowires, with their excellent thermal conductivity, become a key element for improving the thermal conductivity of composite materials. In addition, the use of aluminum-doped silicon carbide nanowires significantly improves the strength of carbon fiber composites by constructing a bamboo-like morphology and improving the intrinsic mechanical properties of nanowires.

[0011] Furthermore, the present invention adopts an innovative PSS-[3-(2-aminoethyl)amino]propyl-substituted heptaisobutyl (CAS: 444315-16-6) modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform, aiming to comprehensively improve the mechanical properties, thermophysical properties of carbon fiber composite materials and the interface compatibility and bonding strength between carbon fiber and polyimide matrix through interface structure design and regulation. First, the introduction of PSS-[3-(2-aminoethyl)amino]propyl-substituted heptaisobutyl can significantly promote the crystallization behavior of polyimide on the surface of aluminum-doped silicon carbide nanowire / carbon fiber composite preform. This specially designed substituent group can induce the polyimide molecular chain to form an orderly arrangement on the surface of the preform through chemical bonding, thereby inducing crystallization. The formation of polyimide crystalline regions can not only improve the bonding strength at the interface, but also improve the transmission and distribution of stress between fibers, nanowires and matrix, thereby significantly improving the mechanical properties of the composite material, especially strength and toughness. Secondly, the presence of PSS-[3-(2-aminoethyl)amino]propyl-substituted heptaisobutyl can significantly improve the interfacial compatibility between the aluminum-doped silicon carbide nanowire / carbon fiber composite preform and the polyimide matrix. This substituted group can form secondary interactions such as hydrogen bonds with the polyimide molecular chain to increase the adhesion at the interface. Good interfacial compatibility is conducive to achieving stress transfer and synergistic reinforcement between the fiber, nanowire and matrix, avoiding early failure caused by interface debonding, delamination, etc. In addition, the improved interfacial compatibility can also promote the homogenization of the internal stress state of the composite material, improve the fatigue resistance and service life of the material. More importantly, the uniform distribution of polyimide crystalline regions on the surface of the aluminum-doped silicon carbide nanowire / carbon fiber composite preform can form a unique strong-plastic matching structure. The crystalline region, as a reinforcing phase, can provide excellent strength and stiffness; the non-crystalline region, as a plastic matrix, gives the material good toughness and ductility. This strong-plastic matching structure can effectively balance the strength and toughness of the composite material and achieve synergistic optimization of high strength and high toughness. At the same time, the presence of the crystalline region can also improve the thermophysical properties of the composite material, such as increasing thermal conductivity, reducing thermal expansion coefficient, etc., which is crucial for high-temperature application environments such as aerospace. In summary, the present invention adopts PSS-[3-(2-aminoethyl)amino]propyl-substituted heptaisobutyl modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform, which significantly improves its thermophysical properties while improving the mechanical properties of the composite material by promoting polyimide crystallization, improving interface compatibility, and constructing a strong-plastic matching structure. This multi-scale, multi-level interface structure regulation strategy provides a new idea for the design and preparation of high-performance carbon fiber composites, and is expected to promote the wide application and technological innovation of carbon fiber composites in the fields of aerospace, high-end equipment manufacturing, etc.

[0012] At the same time, the polyimide resin matrix obtained after curing the polyamic acid mixed solution also provides a good heat conduction path as a continuous phase, and works synergistically with the silicon carbide nanowires to jointly improve the thermal management capability of the composite material.

[0013] Furthermore, the aluminum-doped silicon carbide nanowires have a bamboo-like morphology and are uniformly distributed on the surface of the carbon fiber preform in a divergent manner in an in-situ growth manner.

[0014] The silicon carbide nanowires designed by the present invention are designed to be bamboo-shaped and are evenly distributed on the surface of carbon fiber in a divergent manner in an in-situ growth manner. The purpose is: 1) The bamboo-shaped aluminum-doped silicon carbide nanowires, with their unique morphology, not only increase the contact area with the surface of the silicon carbide nanowires, but also provide an additional mechanical locking effect through their node structure; this locking effect effectively prevents interface slip and crack propagation, and significantly enhances the interface bonding force between the aluminum-doped silicon carbide nanowires and the polyimide resin matrix. 2) The bamboo-shaped structure not only increases the specific surface area of ​​the nanowires, but also forms more heat conduction channels; these channels are evenly distributed in a divergent manner on the surface of the carbon fiber, constructing an efficient three-dimensional heat conduction network; when heat is transferred in the composite material, these networks can quickly disperse and export the heat, thereby significantly improving the thermal conductivity of the material. 3) The bamboo-like morphology of aluminum-doped silicon carbide nanowires can not only greatly increase the specific surface area of ​​the nanowires and provide more interface binding sites, but also introduce stress concentration effects and activate strengthening mechanisms such as dislocations and grain boundaries; the bamboo-like structure can effectively hinder the movement of dislocations and increase the storage density of dislocations, thereby significantly enhancing the strength of the nanowires. Compared with conventional smooth nanowires, the strength of bamboo-like aluminum-doped silicon carbide nanowires is significantly improved.

[0015] In summary, the present invention has successfully improved the comprehensive performance of carbon fiber skin materials in terms of strength, expansion coefficient, thermal conductivity, etc. by further designing the specific morphology and distribution of aluminum-doped silicon carbide nanowires and combining the excellent performance of the polyimide resin matrix. This innovative design not only broadens the application field of carbon fiber composite materials, but also provides a more reliable and efficient material solution for the field of high-end equipment manufacturing.

[0016] Furthermore, the interface between the carbon fiber preform and the aluminum-doped silicon carbide nanowires is a semi-coherent interface.

[0017] The present invention introduces silicon carbide nanowires on the surface of carbon fiber and carefully designs the interface structure between carbon fiber and silicon carbide nanowires, aiming to significantly improve the mechanical properties and thermophysical properties of the composite material. The semi-coherent interface design is adopted between the carbon fiber and the silicon carbide nanowire of the present invention. This unique interface structure can improve the material properties from multiple aspects. First, the semi-coherent interface can greatly improve the bonding strength between the carbon fiber and the silicon carbide nanowire. In the semi-coherent interface, the carbon fiber and the silicon carbide nanowire form a regular atomic arrangement and bonding mode at the atomic scale, so that a strong chemical bonding effect is formed between the two phases. This strong chemical bonding can not only effectively transfer the load, but also inhibit the slip and debonding phenomenon at the interface, thereby significantly improving the strength and toughness of the composite material. Compared with the conventional non-coherent interface, the bonding strength of the semi-coherent interface significantly improves the interface bonding strength. Secondly, the semi-coherent interface is conducive to improving the phonon transmission efficiency between the carbon fiber and the silicon carbide nanowire, and improving the thermal conductivity of the composite material. In the semi-coherent interface, since the lattice constants of the two-phase materials have a certain matching relationship, the phonon scattering and reflection at the interface are effectively suppressed, forming a "phonon transmission channel". This special interface structure can significantly reduce the energy loss of phonons at the interface, promote the efficient transmission of phonons between carbon fiber and silicon carbide nanowires, and thus greatly improve the thermal conductivity of the composite material. High thermal conductivity is not only conducive to the rapid dissipation of heat inside the material, reducing the risk of damage caused by thermal stress, but also can improve the performance and reliability of the composite material in high temperature environment. In addition, the semi-coherent interface also has a unique stress distribution and transfer mechanism. Because the atomic arrangement at the interface is more orderly, stress can be transmitted along a specific crystal plane and direction, achieving uniform dispersion of stress between nanowires and fibers. This stress distribution mechanism can effectively avoid early failure caused by stress concentration and improve the fatigue resistance and service life of the composite material. In summary, the present invention achieves a comprehensive improvement in the mechanical properties and thermophysical properties of the composite material by introducing silicon carbide nanowires on the surface of carbon fiber and adopting a semi-coherent interface design. The semi-coherent interface not only greatly enhances the bonding strength between carbon fiber and silicon carbide nanowires, but also significantly improves the phonon transmission efficiency and stress distribution characteristics at the interface, bringing revolutionary improvements to the strength, toughness, thermal conductivity and reliability of the composite material. This high-performance carbon fiber composite material is expected to be widely used in fields such as aerospace, high-end equipment manufacturing, etc. that have extremely high requirements for material performance, leading the innovative development of material technology.

[0018] Furthermore, the aluminum-doped silicon carbide nanowires have an average diameter of 20 to 80 nm and an average length of 20 to 100 μm.

[0019] Furthermore, the preparation method of the surface modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform comprises the following steps: adding 2 to 4 parts of PSS-[3-(2-aminoethyl)amino]propyl-substituted heptaisobutyl and 40 to 60 parts of N-methylpyrrolidone into a container, first ultrasonically treating for 15 to 25 minutes, and then magnetically stirring for 15 to 24 hours to obtain a uniform mixed solution, and then immersing 6 to 12 parts of the aluminum-doped silicon carbide nanowire / carbon fiber composite preform in the uniform mixed solution, followed by ultrasonic immersion for 5 to 10 minutes, and finally taking it out and drying it in a vacuum drying oven at room temperature for 18 to 24 hours to obtain a surface modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform.

[0020] Furthermore, the preparation method of the aluminum-doped silicon carbide nanowire / carbon fiber composite preform comprises the following steps: after uniformly mixing 20 to 40 parts of polycarbosilane, 0.5 to 0.8 parts of aluminum nitrate, 1 to 3 parts of nickel nitrate and 100 parts of ethanol by weight, 5 to 9 parts of carbon fiber preforms are completely impregnated therein for 10 to 25 minutes. After the impregnation is completed, the preforms are placed in a vacuum drying oven and dried for 12 to 24 hours. After the impregnated fiber preforms are dried, they are placed in a vertical vacuum furnace, heated to 1200 to 1400°C in an argon atmosphere, kept warm for 2 to 5 hours, and cooled to room temperature to obtain an aluminum-doped silicon carbide nanowire / carbon fiber composite preform.

[0021] The present invention introduces aluminum-doped silicon carbide nanowires on the surface of a carbon fiber preform, aiming to further improve the mechanical properties, especially the strength, of carbon fiber composite materials through morphology control and component design of the nanowires. By introducing aluminum elements into silicon carbide nanowires, the growth behavior and morphological characteristics of the nanowires can be significantly changed; the incorporation of aluminum atoms can induce silicon carbide nanowires to form a unique bamboo-like structure. And aluminum doping can also improve the intrinsic mechanical properties of silicon carbide nanowires. The introduction of aluminum atoms can cause the silicon carbide lattice to distort, forming defect structures such as point defects and dislocations. These defects can act as pinning points for dislocations, hindering the slip and movement of dislocations, thereby improving the strength of the nanowires.

[0022] In summary, the present invention performs aluminum doping on silicon carbide nanowires, which not only induces silicon carbide nanowires to form high-strength bamboo-like structures, but also further enhances the mechanical properties of nanowires by introducing defects and other mechanisms. In addition, the excellent interface bonding formed between aluminum-doped silicon carbide nanowires and carbon fibers can effectively transfer loads and improve the toughness and impact resistance of composite materials. This multi-scale synergistic enhancement strategy provides new ideas for the design of high-strength and high-toughness carbon fiber composites, and is expected to promote their application and development in aerospace and other fields.

[0023] Furthermore, the mass ratio of the polycarbosilane to aluminum nitrate is (40-50):1.

[0024] Furthermore, the aluminum doping amount in the aluminum-doped silicon carbide nanowires is 0.5 at % to 2.5 at %.

[0025] Furthermore, the polyamic acid mixed solution is prepared from the following raw materials in parts by weight: 20 to 30 parts of p-phenylenediamine, 54 to 81 parts of 3,3',4,4'-biphenyltetracarboxylic dianhydride, 100 parts of dimethylacetamide, 2 to 5 parts of 1,8-diamino-3,6-dioxaoctane, and 3 to 7 parts of diphenylmethane-4,4'-diisocyanate.

[0026] Furthermore, the preparation method of the polyamic acid mixed solution comprises the following steps: in an argon atmosphere, p-phenylenediamine, 3,3',4,4'-biphenyltetracarboxylic dianhydride and dimethylacetamide are uniformly mixed, stirred at -10°C to -5°C for 10 to 20 hours, and then 1,8-diamino-3,6-dioxaoctane and diphenylmethane-4,4'-diisocyanate are added, and stirring is continued for 6 to 10 hours to obtain the polyamic acid mixed solution.

[0027] Furthermore, the mass ratio of p-phenylenediamine to 3,3',4,4'-biphenyltetracarboxylic dianhydride is 1:2.7.

[0028] The present invention adopts a unique polyamic acid mixed solution formula, and through the careful design of monomer types and dosages, it aims to give carbon fiber composite materials excellent self-healing ability and significantly improve their service life and reliability. The self-healing polyimide of the present invention forms a cross-linked structure by introducing a flexible segment 1,8-diamino-3,6-dioxaoctane with a rigid polyimide main chain, and uses the flexible segment to give the polymer molecular chain a certain mobility, so that the material can re-establish intermolecular interactions when damaged to achieve self-healing. At the same time, diphenylmethane-4,4'-diisocyanate is used to form a urea-based cross-linked structure with polyimide, which improves the strength, elastic modulus and toughness of the polyimide. In addition, dimethylacetamide is used as a solvent to form a uniform mixed solution of polyimide, optimize the solution concentration and viscosity, and help prepare high-quality self-healing polyimide materials. By adjusting the feeding ratio of monomers, especially flexible segments and isocyanates, the chemical structure and cross-linking density of polyimide can be optimized, and the controllable preparation of polyimide with excellent self-healing properties and mechanical properties can be achieved.

[0029] Furthermore, the carbon fiber preform is a carbon fiber preform that is braided with carbon fibers in a 2.5D weaving or 3D weaving manner according to the shape of the skin.

[0030] The present invention also provides a method for preparing a high-strength carbon fiber skin material, comprising the following steps:

[0031] S1, impregnation: placing the surface-modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform into a mold, then adding the polyamic acid mixed solution and ultrasonically impregnating for 20 to 35 minutes;

[0032] S2, curing and molding: the mold is first kept at 50°C for 10 to 16 hours, then heated to 120°C and kept at 3 to 6 hours, and finally kept at 260°C for 2 to 5 hours, and the polyamic acid mixed solution is cured to obtain polyimide, thereby preparing the high-strength carbon fiber skin material.

[0033] The invention also discloses application of a high-strength carbon fiber skin material, wherein the high-strength carbon fiber skin material is used for a wing structure.

[0034] (3) Beneficial technical effects

[0035] 1. The present invention constructs a hierarchical structure and a multi-scale reinforcement mechanism by loading silicon carbide nanowires on the surface of a carbon fiber preform, thereby enhancing and optimizing the performance of the carbon fiber skin material from multiple microscopic and macroscopic levels. The introduction of silicon carbide nanowires, on the one hand, significantly increases the contact area between the fiber and the matrix, forms a mechanical interlocking structure, and forms a chemical bond with the polyimide matrix, thereby improving the interface bonding strength and inhibiting interface stratification and damage; on the other hand, silicon carbide nanowires, as the second reinforcement phase, form a nanoscale reinforcement network in the matrix, hinder crack propagation, absorb and dissipate external force energy, and improve the strength, modulus and toughness of the composite material. In addition, the excellent high temperature resistance, wear resistance, corrosion resistance and other properties of silicon carbide nanowires, as well as certain electrical and thermal conductivity properties, give the composite material multifunctional characteristics and broaden its application range. The present invention adopts an in-situ growth method to introduce silicon carbide nanowires, simplifies the process flow, and improves the machinability and molding quality of the composite material. Through the modification of silicon carbide nanowires, the present invention endows the carbon fiber skin material with more excellent comprehensive performance, making it suitable for key components and structural parts with higher requirements on material performance. It has significant innovation and practicality, and provides new ideas and methods for the design and preparation of high-performance composite materials.

[0036] 2. The present invention adopts PSS-[3-(2-aminoethyl)amino]propyl-substituted heptaisobutyl modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform, which comprehensively improves the mechanical and thermophysical properties of the composite material by promoting polyimide crystallization, enhancing interface compatibility and constructing a strong-plastic matching structure, thereby achieving high strength, high toughness and excellent thermal management performance.

[0037] 3. The bamboo-shaped silicon carbide nanowires designed by the present invention are evenly distributed on the surface of carbon fiber in an in-situ growth mode, achieving multiple beneficial effects: enhancing the interface bonding force, inhibiting interface slip and crack propagation through morphology and node structure; optimizing thermal expansion behavior, forming a thermal stress buffer layer, and reducing the thermal expansion coefficient; improving thermal conductivity, building an efficient three-dimensional heat conduction network, and accelerating heat dispersion and extraction. Comprehensively improve the strength, thermal expansion resistance and thermal conductivity of carbon fiber composite materials, broaden their application range, and provide excellent material support for high-end equipment.

[0038] 4. The present invention introduces silicon carbide nanowires on carbon fiber and adopts a semi-coherent interface design to significantly improve the mechanical and thermophysical properties of the composite material: strengthen interface bonding to achieve efficient load transfer and anti-slip; optimize phonon transmission, enhance thermal conductivity, and promote rapid heat dissipation; improve stress distribution and enhance fatigue resistance.

[0039] 5. The present invention introduces aluminum-doped silicon carbide nanowires on the surface of carbon fiber, forms a high-strength bamboo-like structure by regulating the morphology and components, and improves the intrinsic mechanical properties of the nanowires, significantly improving the strength of the composite material. The bamboo-like morphology induced by aluminum doping and the defective structure work together to enhance the strength of the nanowires, while optimizing the interface bonding, improving the toughness and impact resistance of the composite material, and providing a new path for the design of high-strength and high-toughness carbon fiber composite materials.

[0040] 6. The present invention adopts a unique polyamic acid mixed solution formula, and by fusing flexible segments with rigid polyimide, a cross-linked structure is constructed to give carbon fiber composites self-healing ability, significantly improving durability and reliability. The flexible segments enhance the mobility of the molecular chain and promote self-healing of damage; the isocyanate enhances the strength, modulus and toughness of the material. The solvent optimizes the solution properties, accurately controls the monomer ratio, and realizes the controllable preparation of high-performance self-healing polyimide, expanding the application prospects of carbon fiber composites.

[0041] 7. The present invention not only designs a high-performance carbon fiber composite material with self-healing ability, but also applies it to the protection of the outer surface of the wing structure as a high-strength carbon fiber skin material. This application significantly improves the durability, damage resistance and overall performance of the wing structure, extends the service life, and enhances the safety and reliability of the structure. This innovative application provides important technical support for the fields of aerospace and high-end equipment, and promotes the progress and development of materials science. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 This is a SEM morphology image of the bamboo-shaped aluminum-doped silicon carbide nanowires prepared in Example 1 of the present invention.

[0043] Figure 2 This is a SEM morphology image of the aluminum-doped silicon carbide nanowire / carbon fiber composite preform prepared in Example 1 of the present invention.

[0044] Figure 3 This is a TEM electron microscope image of the interface between the carbon fiber preform and the silicon carbide nanowires prepared in Example 1 of the present invention.

[0045] Figure 4 This is a phase analysis diagram of the aluminum-doped silicon carbide nanowire / carbon fiber composite preform prepared in Example 1 of the present invention.

[0046] Figure 5 This is a phase analysis diagram of the high-strength carbon fiber skin material prepared in Example 1 of the present invention.

[0047] Figure 6 This is a SEM morphology image of the linear silicon carbide nanowires prepared in Comparative Example 2 of the present invention.

[0048] Figure 7 Phase analysis of the high-strength carbon fiber skin material prepared in Comparative Example 3 of the present invention. DETAILED DESCRIPTION

[0049] To make the purpose, technical solution and advantages of the embodiments of the present invention more clear, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings in the embodiments of the present invention.

[0050] In the case of not specifying specific conditions, the operation in the embodiment is carried out according to conventional conditions or the conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not indicated, are all common products on the market. The parts not mentioned in the technical content of the present invention will be processed with reference to the prior art. Unless otherwise specified, the following examples and comparative examples will be tested in parallel and use the same processing steps and parameters. Table 1 shows the reagents required for the examples and comparative examples and the corresponding purchasing companies.

[0051] Table 1 Reagents required for the examples and comparative examples and the corresponding purchasing companies

[0052]

[0053] Example 1

[0054] A high-strength carbon fiber skin material is prepared from the following raw materials in parts by weight: 30 parts of a surface-modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform and 40 parts of a polyamic acid mixed solution.

[0055] The surface-modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform is prepared by surface-modifying the aluminum-doped silicon carbide nanowire / carbon fiber composite preform with PSS-[3-(2-aminoethyl)amino]propyl-substituted heptaisobutyl; the aluminum-doped silicon carbide nanowire / carbon fiber composite preform comprises a carbon fiber preform and aluminum-doped silicon carbide nanowires loaded on the surface of the carbon fiber preform.

[0056] The interface between the carbon fiber preform and the aluminum-doped silicon carbide nanowires is a semi-coherent interface; the morphology of the aluminum-doped silicon carbide nanowires is bamboo-node-shaped, and they are evenly distributed on the surface of the carbon fiber preform in a divergent manner in an in-situ growth manner; the average diameter of the aluminum-doped silicon carbide nanowires is 20nm, the average length is 25μm, and the aluminum doping amount in the aluminum-doped silicon carbide nanowires is 2.5at%.

[0057] The polyamic acid mixed solution is prepared from the following raw materials in parts by weight: 20 parts of p-phenylenediamine, 54 parts of 3,3',4,4'-biphenyltetracarboxylic dianhydride, 100 parts of dimethylacetamide, 2 parts of 1,8-diamino-3,6-dioxaoctane, and 3 parts of diphenylmethane-4,4'-diisocyanate.

[0058] The preparation method of the surface modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform comprises the following steps:

[0059] S1: In terms of weight, 20 parts of polycarbosilane, 0.5 parts of aluminum nitrate, 1 part of nickel nitrate and 100 parts of ethanol were mixed evenly, and 5 parts of 2.5D woven carbon fiber preforms were completely impregnated therein for 10 minutes. After the impregnation, the preforms were placed in a vacuum drying oven and dried for 12 hours. After the impregnated fiber preforms were dried, they were placed in a vertical vacuum furnace and heated to 1200°C in an argon atmosphere. The preforms were kept warm for 2 hours and cooled to room temperature to obtain aluminum-doped silicon carbide nanowire / carbon fiber composite preforms.

[0060] S2: Add 2 parts of PSS-[3-(2-aminoethyl)amino]propyl-substituted heptaisobutyl and 40 parts of N-methylpyrrolidone into a container, first ultrasonically treat for 15 minutes, and then magnetically stir for 15 hours to obtain a uniform mixed solution, then 6 parts of aluminum-doped silicon carbide nanowire / carbon fiber composite preform are immersed in the uniform mixed solution, followed by ultrasonic immersion for 5 minutes, and finally taken out and dried in a vacuum drying oven at room temperature for 18 hours to obtain a surface-modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform.

[0061] The method for preparing the high-strength carbon fiber skin material in this embodiment includes the following steps:

[0062] S1. Preparing a polyamic acid mixed solution: in an argon atmosphere, p-phenylenediamine, 3,3',4,4'-biphenyltetracarboxylic dianhydride and dimethylacetamide were uniformly mixed, and the mixture was stirred at -10°C for 10 hours, and then 1,8-diamino-3,6-dioxaoctane and diphenylmethane-4,4'-diisocyanate were added, and the mixture was stirred for 6 hours to obtain the polyamic acid mixed solution;

[0063] S2, impregnation: placing the surface modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform into a mold, then adding the polyamic acid mixed solution and ultrasonically impregnating for 20 minutes;

[0064] S3, curing and molding: the mold is first kept at 50° C. for 10 hours, then heated to 120° C. and kept at that temperature for 3 hours, and finally kept at 260° C. for 2 hours to prepare the high-strength carbon fiber skin material.

[0065] Example 2

[0066] A high-strength carbon fiber skin material is prepared from the following raw materials in parts by weight: 39 parts of a surface-modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform and 49 parts of a polyamic acid mixed solution.

[0067] The surface-modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform is prepared by surface-modifying the aluminum-doped silicon carbide nanowire / carbon fiber composite preform with PSS-[3-(2-aminoethyl)amino]propyl-substituted heptaisobutyl; the aluminum-doped silicon carbide nanowire / carbon fiber composite preform comprises a carbon fiber preform and aluminum-doped silicon carbide nanowires loaded on the surface of the carbon fiber preform.

[0068] The interface between the carbon fiber preform and the aluminum-doped silicon carbide nanowires is a semi-coherent interface; the morphology of the aluminum-doped silicon carbide nanowires is bamboo-node-shaped, and they are evenly distributed on the surface of the carbon fiber preform in a divergent manner in an in-situ growth manner; the average diameter of the aluminum-doped silicon carbide nanowires is 38nm, and the average length is 42μm; the aluminum doping amount in the aluminum-doped silicon carbide nanowires is 2.0at%.

[0069] The polyamic acid mixed solution is prepared from the following raw materials in parts by weight: 23 parts of p-phenylenediamine, 62 parts of 3,3',4,4'-biphenyltetracarboxylic dianhydride, 100 parts of dimethylacetamide, 3 parts of 1,8-diamino-3,6-dioxaoctane, and 4 parts of diphenylmethane-4,4'-diisocyanate.

[0070] The preparation method of the surface modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform comprises the following steps:

[0071] S1: In terms of weight, 26 parts of polycarbosilane, 0.6 parts of aluminum nitrate, 2 parts of nickel nitrate and 100 parts of ethanol were mixed evenly, and 6 parts of 3D woven carbon fiber preforms were completely impregnated therein for 15 minutes. After the impregnation, the preforms were placed in a vacuum drying oven and dried for 17 hours. After the impregnated fiber preforms were dried, they were placed in a vertical vacuum furnace and heated to 1260°C in an argon atmosphere. The preforms were kept warm for 3 hours and cooled to room temperature to obtain aluminum-doped silicon carbide nanowire / carbon fiber composite preforms.

[0072] S2: 3 parts of PSS-[3-(2-aminoethyl)amino]propyl-substituted heptaisobutyl and 46 parts of N-methylpyrrolidone were added into a container and ultrasonically treated for 18 minutes, and then magnetically stirred for 18 hours to obtain a uniform mixed solution. Then, 8 parts of aluminum-doped silicon carbide nanowire / carbon fiber composite preform were immersed in the uniform mixed solution, followed by ultrasonic immersion for 7 minutes. Finally, it was taken out and dried in a vacuum drying oven at room temperature for 20 hours to obtain a surface-modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform.

[0073] The method for preparing the high-strength carbon fiber skin material in this embodiment includes the following steps:

[0074] S1. Preparing a polyamic acid mixed solution: in an argon atmosphere, uniformly mixing p-phenylenediamine, 3,3',4,4'-biphenyltetracarboxylic dianhydride and dimethylacetamide, stirring at -8°C for 13 hours, then adding 1,8-diamino-3,6-dioxaoctane and diphenylmethane-4,4'-diisocyanate, and continuing stirring for 8 hours to obtain the polyamic acid mixed solution;

[0075] S2, impregnation: placing the surface modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform into a mold, then adding the polyamic acid mixed solution and ultrasonically impregnating for 25 minutes;

[0076] S3, curing and molding: the mold is first kept at 50° C. for 12 hours, then heated to 120° C. and kept at that temperature for 4 hours, and finally kept at 260° C. for 3 hours to prepare the high-strength carbon fiber skin material.

[0077] Example 3

[0078] A high-strength carbon fiber skin material is prepared from the following raw materials in parts by weight: 46 parts of a surface-modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform and 58 parts of a polyamic acid mixed solution.

[0079] The surface-modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform is prepared by surface modification of the aluminum-doped silicon carbide nanowire / carbon fiber composite preform with PSS-[3-(2-aminoethyl)amino]propyl-substituted heptaisobutyl; the aluminum-doped silicon carbide nanowire / carbon fiber composite preform comprises a carbon fiber preform and an aluminum-doped silicon carbide nanowire loaded on the surface of the carbon fiber preform; the interface between the carbon fiber preform and the aluminum-doped silicon carbide nanowire is a semi-coherent interface; the morphology of the aluminum-doped silicon carbide nanowire is bamboo-node-shaped and is uniformly distributed on the surface of the carbon fiber preform in a divergent manner in an in-situ growth manner; the average diameter of the aluminum-doped silicon carbide nanowire is 56nm, the average length is 70μm, and the aluminum doping amount in the aluminum-doped silicon carbide nanowire is 1.0at%.

[0080] The polyamic acid mixed solution is prepared from the following raw materials in parts by weight: 27 parts of p-phenylenediamine, 72 parts of 3,3',4,4'-biphenyltetracarboxylic dianhydride, 100 parts of dimethylacetamide, 4 parts of 1,8-diamino-3,6-dioxaoctane, and 5 parts of diphenylmethane-4,4'-diisocyanate.

[0081] The preparation method of the surface-modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform comprises the following steps:

[0082] S1: In terms of weight, 32 parts of polycarbosilane, 0.7 parts of aluminum nitrate, 2 parts of nickel nitrate and 100 parts of ethanol were mixed evenly, and 8 parts of 2.5D woven carbon fiber preforms were completely impregnated therein for 19 minutes. After the impregnation, the preforms were placed in a vacuum drying oven and dried for 19 hours. After the impregnated fiber preforms were dried, they were placed in a vertical vacuum furnace and heated to 1320°C in an argon atmosphere. The preforms were kept warm for 4 hours and cooled to room temperature to obtain aluminum-doped silicon carbide nanowire / carbon fiber composite preforms.

[0083] S2: 3 parts of PSS-[3-(2-aminoethyl)amino]propyl-substituted heptaisobutyl and 52 parts of N-methylpyrrolidone were added into a container and ultrasonically treated for 21 minutes, and then magnetically stirred for 20 hours to obtain a uniform mixed solution. Then, 10 parts of aluminum-doped silicon carbide nanowire / carbon fiber composite preform were immersed in the uniform mixed solution, followed by ultrasonic immersion for 8 minutes, and finally taken out and dried in a vacuum drying oven at room temperature for 22 hours to obtain a surface-modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform.

[0084] The method for preparing the high-strength carbon fiber skin material in this embodiment includes the following steps:

[0085] S1. Prepare a polyamic acid mixed solution: in an argon atmosphere, mix p-phenylenediamine, 3,3',4,4'-biphenyltetracarboxylic dianhydride and dimethylacetamide evenly, stir at -7°C for 16 hours, then add 1,8-diamino-3,6-dioxaoctane and diphenylmethane-4,4'-diisocyanate, and continue stirring for 9 hours to obtain the polyamic acid mixed solution;

[0086] S2, impregnation: placing the surface modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform into a mold, then adding the polyamic acid mixed solution and ultrasonically impregnating for 28 minutes;

[0087] S3, curing and molding: the mold is first kept at 50° C. for 13 hours, then heated to 120° C. and kept at that temperature for 5 hours, and finally kept at 260° C. for 4 hours to prepare the high-strength carbon fiber skin material.

[0088] Example 4

[0089] A high-strength carbon fiber skin material is prepared from the following raw materials in parts by weight: 55 parts of a surface-modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform and 70 parts of a polyamic acid mixed solution.

[0090] The surface-modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform is prepared by surface-modifying the aluminum-doped silicon carbide nanowire / carbon fiber composite preform with PSS-[3-(2-aminoethyl)amino]propyl-substituted heptaisobutyl; the aluminum-doped silicon carbide nanowire / carbon fiber composite preform comprises a carbon fiber preform and aluminum-doped silicon carbide nanowires loaded on the surface of the carbon fiber preform.

[0091] The interface between the carbon fiber preform and the aluminum-doped silicon carbide nanowires is a semi-coherent interface; the morphology of the aluminum-doped silicon carbide nanowires is bamboo-node-shaped, and they are evenly distributed on the surface of the carbon fiber preform in a divergent manner in an in-situ growth manner; the average diameter of the aluminum-doped silicon carbide nanowires is 80nm, and the average length is 100μm; the aluminum doping amount in the aluminum-doped silicon carbide nanowires is 0.5at%.

[0092] The polyamic acid mixed solution is prepared from the following raw materials in parts by weight: 30 parts of p-phenylenediamine, 81 parts of 3,3',4,4'-biphenyltetracarboxylic dianhydride, 100 parts of dimethylacetamide, 5 parts of 1,8-diamino-3,6-dioxaoctane, and 7 parts of diphenylmethane-4,4'-diisocyanate.

[0093] The preparation method of the surface-modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform comprises the following steps:

[0094] S1: In terms of weight, 40 parts of polycarbosilane, 0.8 parts of aluminum nitrate, 3 parts of nickel nitrate and 100 parts of ethanol were mixed evenly, and 9 parts of 3D woven carbon fiber preforms were completely impregnated therein for 25 minutes. After the impregnation, the preforms were placed in a vacuum drying oven and dried for 24 hours. After the impregnated fiber preforms were dried, they were placed in a vertical vacuum furnace and heated to 1400°C in an argon atmosphere. The preforms were kept warm for 5 hours and cooled to room temperature to obtain aluminum-doped silicon carbide nanowire / carbon fiber composite preforms.

[0095] S2: 4 parts of PSS-[3-(2-aminoethyl)amino]propyl-substituted heptaisobutyl and 60 parts of N-methylpyrrolidone were added into a container and ultrasonically treated for 25 minutes, and then magnetically stirred for 24 hours to obtain a uniform mixed solution. Then, 12 parts of aluminum-doped silicon carbide nanowire / carbon fiber composite preform were immersed in the uniform mixed solution, followed by ultrasonic immersion for 10 minutes, and finally taken out and dried in a vacuum drying oven at room temperature for 24 hours to obtain a surface-modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform.

[0096] The method for preparing the high-strength carbon fiber skin material in this embodiment includes the following steps:

[0097] S1. Preparing a polyamic acid mixed solution: in an argon atmosphere, uniformly mixing p-phenylenediamine, 3,3',4,4'-biphenyltetracarboxylic dianhydride and dimethylacetamide, stirring at -5°C for 20 hours, then adding 1,8-diamino-3,6-dioxaoctane and diphenylmethane-4,4'-diisocyanate, and continuing stirring for 10 hours to obtain the polyamic acid mixed solution;

[0098] S2, impregnation: placing the surface modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform into a mold, then adding the polyamic acid mixed solution and ultrasonically impregnating for 35 minutes;

[0099] S3, curing and molding: the mold is first kept at 50° C. for 16 hours, then heated to 120° C. and kept at that temperature for 6 hours, and finally kept at 260° C. for 5 hours to prepare the high-strength carbon fiber skin material.

[0100] Example 5

[0101] It is basically the same as Example 1, except that the number of the surface-modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform is 42 parts.

[0102] Comparative Example 1

[0103] It is basically the same as Example 1, except that the surface-modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform is replaced by a surface-modified carbon fiber preform.

[0104] The preparation method of a surface-modified carbon fiber preform comprises the following steps: adding 2 parts of PSS-[3-(2-aminoethyl)amino]propyl-substituted heptaisobutyl and 40 parts of N-methylpyrrolidone into a container, firstly ultrasonically treating for 15 minutes, and then magnetically stirring for 15 hours to obtain a uniform mixed solution, and then completely immersing 6 parts of 2.5D woven carbon fiber preforms therein, followed by ultrasonic immersion for 5 minutes, and finally taking it out and drying it in a vacuum drying oven at room temperature for 18 hours to obtain a surface-modified carbon fiber preform.

[0105] Comparative Example 2

[0106] It is basically the same as Example 1, except that the surface-modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform is replaced by a surface-modified silicon carbide nanowire / carbon fiber composite preform.

[0107] The preparation method of the surface-modified silicon carbide nanowire / carbon fiber composite preform comprises the following steps:

[0108] S1: After 20 parts of polycarbosilane, 1 part of nickel nitrate and 100 parts of ethanol are evenly mixed, 5 parts of 2.5D woven carbon fiber preforms are completely impregnated therein for 10 minutes. After the impregnation is completed, the preforms are placed in a vacuum drying oven and dried for 12 hours. After the impregnated fiber preforms are dried, they are placed in a vertical vacuum furnace and heated to 1200°C in an argon atmosphere. The preforms are kept warm for 2 hours and cooled to room temperature to obtain a silicon carbide nanowire / carbon fiber composite preform.

[0109] S2: Add 2 parts of PSS-[3-(2-aminoethyl)amino]propyl-substituted heptaisobutyl and 40 parts of N-methylpyrrolidone into a container, first ultrasonically treat for 15 minutes, and then magnetically stir for 15 hours to obtain a uniform mixed solution, then 6 parts of silicon carbide nanowire / carbon fiber composite preform are immersed in the uniform mixed solution, followed by ultrasonic immersion for 5 minutes, and finally taken out and dried in a vacuum drying oven at room temperature for 18 hours to obtain a surface-modified silicon carbide nanowire / carbon fiber composite preform.

[0110] Comparative Example 3

[0111] It is basically the same as Example 1, except that the surface-modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform is replaced by an aluminum-doped silicon carbide nanowire / carbon fiber composite preform.

[0112] Comparative Example 4

[0113] Basically the same as Example 1, basically the same as Example 1, except that the surface modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform is replaced by a material composed of surface modified aluminum-doped silicon carbide nanowires and surface modified carbon fiber preforms in a mass ratio of 1:5; no coherent interface is formed between the carbon fiber and the doped silicon carbide nanowires.

[0114] The preparation method of the surface modified carbon fiber preform is the same as that of Comparative Example 1.

[0115] The preparation method of surface-modified aluminum-doped silicon carbide nanowires comprises the following steps:

[0116] S1: After 20 parts of polycarbosilane, 1 part of nickel nitrate and 100 parts of ethanol are evenly mixed, 5 parts of 2.5D woven carbon fiber preforms are completely impregnated therein for 10 minutes. After the impregnation is completed, the preforms are placed in a vacuum drying oven and dried for 12 hours. After the impregnated fiber preforms are dried, they are placed in a vertical vacuum furnace and heated to 1200°C in an argon atmosphere. The preforms are kept warm for 2 hours and cooled to room temperature to obtain a silicon carbide nanowire / carbon fiber composite preform.

[0117] S2: The aluminum-doped silicon carbide nanowire / carbon fiber composite preform prepared in S1 was heat treated at 450°C for 10 h in an air atmosphere to remove the carbon fibers to obtain aluminum-doped silicon carbide nanowires, which were then washed three times with anhydrous ethanol and then vacuum dried to obtain aluminum-doped silicon carbide nanowires.

[0118] S3: Add 2 parts of PSS-[3-(2-aminoethyl)amino]propyl-substituted heptaisobutyl and 40 parts of N-methylpyrrolidone into a container, first ultrasonically treat for 15 minutes, and then magnetically stir for 15 hours to obtain a uniform mixed solution. Then, the aluminum-doped silicon carbide nanowires obtained in S2 are immersed in the uniform mixed solution, followed by ultrasonic immersion for 5 minutes, and finally taken out and dried in a vacuum drying oven at room temperature for 18 hours to obtain surface-modified aluminum-doped silicon carbide nanowires.

[0119] Comparative Example 5

[0120] The method is basically the same as Example 1, and the difference is that the polyamic acid mixed solution raw material does not contain 1,8-diamino-3,6-dioxaoctane.

[0121] Characterization Tests:

[0122] from Figures 1 to 7 The characterization results can draw the following conclusions: Example 1 of the present invention successfully prepared a high-strength carbon fiber skin material made of a surface-modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform and a polyamic acid mixed solution. Among them, the aluminum-doped silicon carbide nanowire presents a unique bamboo-like morphology (such as Figure 1 ), and evenly distributed on the surface of the carbon fiber preform (as shown Figure 2 A semi-coherent interface is formed between the carbon fiber preform and the aluminum-doped silicon carbide nanowires (as shown in Figure 3 The results of phase analysis confirmed that carbon fiber, silicon carbide (such as Figure 4as shown) and the presence of partially crystalline polyimide (as Figure 5 In contrast, the silicon carbide nanowires prepared in Comparative Example 2 have a typical linear morphology (as shown in Figure 6 As shown); Comparative Example 3 did not use surface modification treatment, resulting in the inability to obtain a crystalline polyimide matrix in the final composite material (such as Figure 7 In summary, the present invention obtains a high-performance carbon fiber skin material with bamboo-like silicon carbide nanowire reinforcement and partial crystallization of polyimide through surface modification and interface design, which shows excellent comprehensive mechanical properties and service potential.

[0123] Performance Test:

[0124] Mechanical properties: The tensile properties of the carbon fiber skin material were tested on the WDW-200E electronic universal testing machine of Jinan Shijin Co., Ltd. The tensile strength and elongation of the test need to be recorded. The test process is strictly in accordance with GB / T1447-2005 "Test method for tensile properties of carbon fiber reinforced plastics". The sample size is 250mm×25mm×2mm, the gauge length is 150mm, and the tensile rate is 2mm / min. At least 5 samples are tested for each sample, and the arithmetic mean is taken as the final result.

[0125] Thermal physical properties: In order to measure the thermal conductivity and thermal expansion coefficient of high-strength carbon fiber skin materials, a laser thermal conductivity meter (LFA467) produced by Netzsch of Germany can be used. This instrument uses laser technology to accurately measure the thermal conductivity and thermal expansion coefficient of materials under controlled conditions.

[0126] Self-healing performance: Rectangular specimens were prepared according to ASTM D3479 / D3479M-19 standards, and fatigue tests were performed at a frequency of 5-10 Hz using a sinusoidal waving load (stress ratio R=0.1). The stress level was set so that the maximum stress was 50% of the static strength. The test was performed at room temperature and the number of load cycles was 10,000 times. After the fatigue test, the tensile strength of the specimens was tested before self-healing treatment. The specimens after the fatigue test were then heated at 80°C for 60 hours for self-healing repair, and the tensile strength of the specimens after self-healing treatment was tested. The tensile strength before and after the above self-healing treatment was used to evaluate the self-healing performance.

[0127] The properties of the carbon fiber skin materials of Examples 1 to 5 and Comparative Examples 1 to 5 are summarized in Table 2.

[0128] Table 2 Performance of carbon fiber skin materials of Examples 1 to 5 and Comparative Examples 1 to 5

[0129]

[0130]

[0131] The main difference between Comparative Example 1 and Example 1 is whether the carbon fiber preform contains aluminum-doped silicon carbide nanowires. It can be seen from Table 2 that aluminum-doped silicon carbide nanowires can significantly improve the mechanical properties and thermal physical properties of carbon fiber skin materials. This is because the bamboo-shaped silicon carbide nanowires designed by the present invention are evenly distributed on the carbon fiber surface in an in-situ growth manner, achieving multiple beneficial effects: enhancing interface bonding, inhibiting interface slip and crack propagation through morphology and node structure; optimizing thermal expansion behavior, forming a thermal stress buffer layer, and reducing the thermal expansion coefficient; improving thermal conductivity, building an efficient three-dimensional heat conduction network, and accelerating heat dispersion and extraction. Comprehensively improve the strength, thermal expansion resistance and thermal conductivity of carbon fiber composite materials, broaden their application range, and provide excellent material support for high-end equipment.

[0132] The main difference between Comparative Example 2 and Example 1 is whether the silicon carbide nanowires include aluminum doping treatment. It can be seen from Table 2 that the silicon carbide nanowires are doped to obtain bamboo-shaped nanowires. Compared with the undoped straight nanowires, the doped nanowires can significantly improve the mechanical properties of the carbon fiber skin material. This is because the present invention introduces aluminum-doped silicon carbide nanowires on the surface of the carbon fiber, forms a high-strength bamboo-shaped structure by regulating the morphology and components, and improves the intrinsic mechanical properties of the nanowires, significantly improving the strength of the composite material. The bamboo-shaped morphology induced by aluminum doping and the defective structure work together to enhance the strength of the nanowires, while optimizing the interface bonding, improving the toughness and impact resistance of the composite material, and providing a new path for the design of high-strength and high-toughness carbon fiber composite materials.

[0133] The main difference between Comparative Example 3 and Example 1 is whether the aluminum-doped silicon carbide nanowire / carbon fiber composite preform is surface treated. It can be seen from Table 2 that the surface-treated aluminum-doped silicon carbide nanowire / carbon fiber composite preform can significantly improve the mechanical properties and thermophysical properties of the carbon fiber skin material. This is because the present invention adopts PSS-[3-(2-aminoethyl)amino]propyl-substituted heptaisobutyl to modify the aluminum-doped silicon carbide nanowire / carbon fiber composite preform, which promotes the crystallization of polyimide, enhances the interface compatibility and constructs a strong-plastic matching structure, thereby comprehensively improving the mechanical and thermophysical properties of the composite material, and achieving high strength, high toughness and excellent thermal management performance.

[0134] The main difference between Comparative Example 4 and Example 1 is whether a coherent interface is formed between the carbon fiber preform and the aluminum-doped silicon carbide nanowires. It can be seen from Table 2 that the formation of a coherent interface between the carbon fiber preform and the doped silicon carbide nanowires can significantly improve the mechanical properties and thermophysical properties of the carbon fiber skin material. This is because the present invention introduces silicon carbide nanowires into the carbon fiber preform and adopts a semi-coherent interface design to significantly improve the mechanical and thermophysical properties of the composite material: strengthen interface bonding to achieve efficient load transfer and anti-slip; optimize phonon transmission, enhance thermal conductivity, and promote rapid heat dissipation; improve stress distribution and enhance fatigue resistance.

[0135] The main difference between Comparative Example 5 and Example 1 is whether 1,8-diamino-3,6-dioxaoctane is included in the raw material of the polyamic acid mixed solution. It can be seen from Table 2 that 1,8-diamino-3,6-dioxaoctane can significantly improve the self-healing ability of the carbon fiber skin material. This is because the present invention adopts a unique polyamic acid mixed solution formula, and constructs a cross-linked structure by fusing flexible segments with rigid polyimide, thereby giving the carbon fiber composite material self-healing ability and significantly improving durability and reliability.

[0136] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that all equivalent structural changes made under the concept of the present invention and using the contents of the present invention specification and drawings should be covered within the scope of protection of the claims of the present invention.

Claims

1. A high-strength carbon fiber skin material, characterized in that: The method is prepared from the following raw materials in parts by weight: 30 to 55 parts of a surface-modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform and 40 to 70 parts of a polyamic acid mixed solution; The surface-modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform is prepared by surface-modifying the aluminum-doped silicon carbide nanowire / carbon fiber composite preform with PSS-[3-(2-aminoethyl)amino]propyl-substituted heptaisobutyl; the aluminum-doped silicon carbide nanowire / carbon fiber composite preform comprises a carbon fiber preform and an aluminum-doped silicon carbide nanowire loaded on the surface of the carbon fiber preform.

2. The high-strength carbon fiber skin material according to claim 1, characterized in that: The aluminum-doped silicon carbide nanowires have a bamboo-like morphology and are evenly distributed on the surface of the carbon fiber preform in a divergent manner in an in-situ growth manner; The interface between the carbon fiber preform and the aluminum-doped silicon carbide nanowire is a semi-coherent interface.

3. The high-strength carbon fiber skin material according to claim 1 or 2, characterized in that: The aluminum-doped silicon carbide nanowires have an average diameter of 20 to 80 nm and an average length of 20 to 100 μm.

4. The high-strength carbon fiber skin material according to claim 1 or 2, characterized in that: The preparation method of the surface modified aluminum doped silicon carbide nanowire / carbon fiber composite preform comprises the following steps: 2 to 4 parts of PSS-[3-(2-aminoethyl)amino]propyl-substituted heptaisobutyl and 40 to 60 parts of N-methylpyrrolidone are added into a container, and ultrasonic treatment is first performed for 15 to 25 minutes, and then magnetic stirring is performed for 15 to 24 hours to obtain a uniform mixed solution, and then 6 to 12 parts of the aluminum doped silicon carbide nanowire / carbon fiber composite preform is immersed in the uniform mixed solution, followed by ultrasonic immersion for 5 to 10 minutes, and finally it is taken out and dried in a vacuum drying oven at room temperature for 18 to 24 hours, and finally the surface modified aluminum doped silicon carbide nanowire / carbon fiber composite preform is obtained.

5. The high-strength carbon fiber skin material according to claim 1 or 2, characterized in that: The preparation method of the aluminum-doped silicon carbide nanowire / carbon fiber composite preform comprises the following steps: after uniformly mixing 20 to 40 parts of polycarbosilane, 0.5 to 0.8 parts of aluminum nitrate, 1 to 3 parts of nickel nitrate and 100 parts of ethanol by weight, 5 to 9 parts of carbon fiber preforms are completely impregnated therein for 10 to 25 minutes. After the impregnation is completed, the preforms are placed in a vacuum drying oven for drying for 12 to 24 hours. After the impregnated fiber preforms are dried, they are placed in a vertical vacuum furnace, heated to 1200 to 1400° C. in an argon atmosphere, kept warm for 2 to 5 hours, and cooled to room temperature to obtain the aluminum-doped silicon carbide nanowire / carbon fiber composite preform.

6. The high-strength carbon fiber skin material according to claim 1 or 2, characterized in that: The polyamic acid mixed solution is prepared from the following raw materials in parts by weight: 20-30 parts of p-phenylenediamine, 54-81 parts of 3,3',4,4'-biphenyltetracarboxylic dianhydride, 100 parts of dimethylacetamide, 2-5 parts of 1,8-diamino-3,6-dioxaoctane, and 3-7 parts of diphenylmethane-4,4'-diisocyanate.

7. The high-strength carbon fiber skin material according to claim 6, characterized in that: The preparation method of the polyamic acid mixed solution comprises the following steps: in an argon atmosphere, p-phenylenediamine, 3,3',4,4'-biphenyltetracarboxylic dianhydride and dimethylacetamide are uniformly mixed, and then stirred at -10°C to -5°C for 10 to 20 hours, and then 1,8-diamino-3,6-dioxaoctane and diphenylmethane-4,4'-diisocyanate are added, and stirring is continued for 6 to 10 hours to obtain the polyamic acid mixed solution.

8. The high-strength carbon fiber skin material according to claim 1 or 2, characterized in that: The carbon fiber preform is a carbon fiber preform that is braided with carbon fibers in a 2.5D weaving or 3D weaving manner according to the shape of the skin.

9. A method for preparing a high-strength carbon fiber skin material as claimed in any one of claims 1 to 8, characterized in that: The following steps are involved: S1, impregnation: placing the surface-modified aluminum-doped silicon carbide nanowire / carbon fiber composite preform into a mold, then adding the polyamic acid mixed solution and ultrasonically impregnating for 20 to 35 minutes; S2. Curing and molding: the mold is first kept at 50° C. for 10 to 16 hours, then heated to 120° C. and kept at that temperature for 3 to 6 hours, and finally kept at 260° C. for 2 to 5 hours to prepare the high-strength carbon fiber skin material.

10. Use of the high-strength carbon fiber skin material according to any one of claims 1 to 8 or the high-strength carbon fiber skin material prepared by the preparation method according to claim 9 in a wing structure.