Carbon-coated fly ash hollow microsphere composite heat insulation filler and preparation method thereof

By covering carbon material on the surface of hollow microbeads and forming a carbon cladding layer, the problem of insufficient thermal insulation performance of fly ash hollow microbeads is solved, and the efficiency of improving thermal insulation performance and resource utilization of industrial waste is achieved. It is suitable for Various thermal insulation application scenarios.

CN118994941APending Publication Date: 2024-11-22SHANGHAI UNIVERSITY OF ELECTRIC POWER
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411051224.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The insulating properties of hollow microbeads separated from fly ash are insufficient, limiting their use in high-end insulation materials or applications requiring higher insulation performance.

Method used

By covering a layer of carbon material on the surface of the hollow microbeads, pyrolysis reaction is used to form a carbon cladding layer, reducing heat conductivity and enhancing mechanical properties and weather resistance, carbon-coated fly ash hollow microbead separator is prepared by coating a layer of carbon-coated fly ash. Hot filler.

Benefits of technology

It significantly improves the thermal insulation performance, is suitable for the field of efficient thermal insulation, realizes the resource utilization of industrial waste, reduces production costs, and is suitable for large-scale industrial production, with stable product quality and is suitable for composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994941A_ABST
    Figure CN118994941A_ABST
Patent Text Reader

Abstract

The preparation method comprises the following steps: mixing anhydrous dextrose, hollow microspheres and distilled water, uniformly stirring to prepare a mixed solution, stopping stirring when no lumps exist in the mixed solution, putting the mixed solution into a reaction kettle, carrying out hydrothermal treatment, and after the reaction is finished, cooling to room temperature to obtain the carbon-coated hollow microsphere heat-insulating filler. And naturally cooling to room temperature, centrifugally collecting a sample, washing the sample with deionized water and absolute ethyl alcohol, and drying to obtain the novel carbon-coated hollow microsphere heat-insulating filler. The preparation method provided by the invention has the beneficial effects that the process is simple and controllable, the operation condition is mild, and the heat conductivity coefficient of the obtained novel filler is 0.068 W / Mk.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of heat-insulating fillers, and in particular to a carbon-coated fly ash hollow microbead composite heat-insulating filler and a preparation method thereof. Background Art

[0002] Hollow microspheres are hollow spherical particles and are one of the most important value-added materials in fly ash. The unique properties of hollow microspheres include light weight, good filling factor, enhanced insulation, improved flow characteristics, low water absorption, high compressive strength, chemical inertness and good heat resistance, which make them widely used in industry. However, the hollow microspheres separated from fly ash are not very ideal. Coating hollow microspheres with carbon can improve the thermal insulation performance of hollow microspheres. Promote the application of fly ash hollow microspheres in thermal insulation fillers.

[0003] Although hollow microspheres in fly ash have many advantages mentioned above, hollow microspheres directly separated from fly ash often have certain limitations in performance, especially their thermal insulation performance may not be ideal. This limits their use in high-end thermal insulation materials or application scenarios that require higher thermal insulation performance. Given the huge amount of fly ash produced in my country each year, which contains a large number of hollow microspheres, in-depth exploration of the properties and applications of fly ash hollow microspheres has important academic and practical significance. Summary of the invention

[0004] In order to overcome the deficiencies of the above-mentioned prior art, the purpose of the invention is to provide a new type of thermal insulation filler of carbon-coated hollow microspheres and a preparation method thereof. By coating a layer of carbon material on the surface of hollow microspheres, their thermal insulation performance can be significantly improved. As an efficient thermal insulation barrier, the carbon layer can further reduce the thermal conductivity of the microspheres, thereby improving the thermal insulation effect of the entire material. In addition, carbon coating may also enhance the mechanical properties, weather resistance and chemical stability of the microspheres, further broadening their scope of application.

[0007] To solve the above technical problems, the technical solutions of the present invention are as follows: On the one hand, the present invention provides a method for preparing a carbon-coated fly ash hollow microsphere thermal insulation filler, which is characterized in that it comprises: Step 1. Dissolve the hollow microspheres in deionized water, and evenly disperse the hollow microspheres in the deionized water by stirring to obtain a suspension A, wherein the mass ratio of the hollow microspheres to the deionized water is 1:(8-10); Step 2. Pour anhydrous glucose into the suspension A obtained in step 1 and stir evenly, so that the glucose molecules are gradually adsorbed on the surface of the hollow microspheres or combined with the hollow microspheres to obtain a mixed solution B, wherein the mass ratio of hollow microspheres to anhydrous glucose is (1.2-1.25):1; Step 3. placing the mixed solution B in a reactor and heating it to cause the glucose molecules to undergo a thermal decomposition reaction to form a carbon coating layer on the surface of the hollow microspheres; Step 4. After the heating reaction is completed, cool to room temperature to obtain sample C; Step 5. Wash the sample C obtained in step 4 several times with deionized water and anhydrous ethanol, and then dry it to obtain a carbon-coated fly ash hollow microsphere thermal insulation filler. Preferably, the hollow microspheres have a particle size of 300-400We. Preferably, the temperature of the reactor is 170-190° C., and the reaction time is 12-24 hours. Preferably, the cleaning is centrifugal cleaning with a rotation speed of 8000-10000 r / min and a time of 5-10 min. Preferably, the drying temperature of the drying treatment is 80-90° C., and the drying time is 24-36 hours. On the other hand, the present invention also provides a carbon-coated fly ash hollow microsphere thermal insulation filler, which is characterized in that the carbon-coated fly ash hollow microsphere thermal insulation filler prepared by the above-mentioned preparation method has a particle size between 40-100um and a thermal insulation coefficient of 0.068W / mK. Compared with the prior art, the present invention has the following beneficial effects: 1) The carbon coating effectively reduces the heat conduction path and enhances the ability to reflect thermal radiation, so that the thermal insulation filler has excellent thermal insulation performance while maintaining its light weight. It is suitable for construction, aerospace, electronic appliances and other fields that require efficient thermal insulation. 2) Using fly ash hollow microspheres as the base material not only realizes the resource utilization of industrial waste, reduces environmental pollution, but also reduces production costs. At the same time, anhydrous glucose as a carbon source has a wide range of sources and good biodegradability, and the entire production process conforms to the concept of green manufacturing. 3) The preparation method of the present invention has simple steps, easy-to-control conditions, does not require complex equipment and high energy consumption processes, and is suitable for large-scale industrial production. In addition, the optimized design of the centrifugal washing and drying steps improves production efficiency and reduces energy consumption. 4) The stability and consistency of product quality are ensured by finely controlling the process parameters. The prepared thermal insulation filler has uniform particle size and excellent thermal insulation performance. It can be widely used in various composite materials that require thermal insulation, such as thermal insulation mortar, thermal insulation coating, thermal insulation board, etc., and has broad market prospects. 5) The present invention improves the thermal insulation of fly ash hollow microspheres, and further studies and develops fly ash hollow microspheres, providing a solid foundation for their future applications in the fields of environmental protection and energy conversion, and showing their broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained by using these drawings without creative labor. Among them:

[0012] Figure 1 This is a SEM image of the carbon-coated hollow microspheres prepared in the present invention.

[0013] Figure 2 This is a graph showing the thermal insulation coefficient of the carbon-coated hollow microspheres prepared in the present invention. DETAILED DESCRIPTION The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.

[0015] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification. Example 1

[0016] 20 g of hollow microspheres were dissolved in 200 ml of deionized water and stirred to obtain a mixed solution A.

[0017] Pour 20 g of anhydrous glucose into mixed solution A and stir evenly to obtain mixed solution B.

[0018] Solution B was placed in a reactor for heating, and sample C was obtained after cooling. Sample C was washed three times with deionized water and anhydrous ethanol, and finally sample C was dried to obtain a novel thermal insulation filler sample 1 of carbon-coated hollow microbeads. Example 2

[0019] 20 g of hollow microspheres were dissolved in 200 ml of deionized water and stirred to obtain a mixed solution A.

[0020] Pour 25 g of anhydrous glucose into mixed solution A and stir evenly to obtain mixed solution B.

[0021] Solution B was placed in a reactor for heating, and sample C was obtained after cooling. Sample C was washed three times with deionized water and anhydrous ethanol, and finally sample C was dried to obtain a novel thermal insulation filler sample 2 of carbon-coated hollow microbeads.

[0022] The obtained carbon-coated hollow microspheres were sent for characterization. As shown in 1, this is the SEM image of sample 2. Figure 1It can be seen that there are many small balls coated on the surface of the hollow microbeads, forming a coating layer. Example 3

[0023] 15 g of hollow microspheres were dissolved in 200 ml of deionized water and stirred to obtain a mixed solution A.

[0024] Pour 20 g of anhydrous glucose into mixed solution A and stir evenly to obtain mixed solution B.

[0025] Solution B was placed in a reactor for heating, and sample C was obtained after cooling. Sample C was washed three times with deionized water and anhydrous ethanol, and finally sample C was dried to obtain a novel thermal insulation filler sample 3 of carbon-coated hollow microbeads. like Figure 2 The following table shows the thermal conductivity of three samples. The ratios of anhydrous glucose to hollow microspheres in samples 1, 2, and 3 are 1:1, 1.25:1, and 0.75:1, respectively. Sample 2 has the best effect, with a thermal conductivity of 0.06891, and is more suitable as a thermal insulation filler to enhance the thermal insulation effect of thermal insulation materials or thermal insulation coatings. Experiments have shown that the present invention uses anhydrous glucose as a carbon source to pyrolyze the hollow microspheres to form a carbon coating layer, which is not only low-cost and easy to operate, but also can effectively improve the thermal insulation performance of the hollow microspheres. Compared with traditional chemical vapor deposition or physical coating methods, it does not require complex equipment and is easy to mass produce. At the same time, the optimal mass ratio between hollow microspheres and deionized water and anhydrous glucose, as well as the precise temperature range, reaction time, cleaning speed and time, drying conditions, etc. of the reactor are adopted. The fine regulation of these parameters ensures the uniformity and density of the carbon coating layer, thereby further improving the thermal insulation effect. By selecting hollow microspheres with a specific particle size range as the substrate and combining the carbon coating technology, the prepared thermal insulation filler has a uniform and small particle size (40-100μm), which is conducive to uniform dispersion in the composite material and improves the overall thermal insulation performance. An extremely low thermal insulation coefficient (0.068W / mK) is achieved, which is significantly better than most traditional thermal insulation materials.

[0026] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.

Claims

1. A method for preparing carbon-coated fly ash hollow microspheres thermal insulation filler, It is characterized in that include: Step 1. Dissolve the hollow microspheres in deionized water, and evenly disperse the hollow microspheres in the deionized water by stirring to obtain a suspension A, wherein the mass ratio of the hollow microspheres to the deionized water is 1:(8-10); Step 2. Pour anhydrous glucose into the suspension A obtained in step 1 and stir evenly, so that the glucose molecules are gradually adsorbed on the surface of the hollow microspheres or combined with the hollow microspheres to obtain a mixed solution B, wherein the mass ratio of hollow microspheres to anhydrous glucose is (1.2-1.25):1; Step 3. placing the mixed solution B in a reactor and heating it to cause the glucose molecules to undergo a thermal decomposition reaction to form a carbon coating layer on the surface of the hollow microspheres; Step 4. After the heating reaction is completed, cool to room temperature to obtain sample C; Step 5. Wash the sample C obtained in step 4 several times with deionized water and anhydrous ethanol, and then dry it to obtain a carbon-coated fly ash hollow microsphere thermal insulation filler.

2. The method for preparing the carbon-coated fly ash hollow microsphere thermal insulation filler according to claim 1, Features: The hollow microspheres have a particle size of 300-400We.

3. The method for preparing the carbon-coated fly ash hollow microsphere thermal insulation filler according to claim 1, Features: The temperature of the reactor is 170-190° C., and the reaction time is 12-24 hours.

4. The method for preparing the carbon-coated fly ash hollow microsphere thermal insulation filler according to claim 1, Features: The cleaning is centrifugal cleaning with a rotation speed of 8000-10000 r / min and a time of 5-10 min.

5. The method for preparing the carbon-coated fly ash hollow microsphere thermal insulation filler according to claim 1, Features: The drying temperature of the drying treatment is 80-90° C., and the drying time is 24-36 hours.

6. A carbon-coated fly ash hollow microsphere thermal insulation filler, It is characterized in that The method is obtained by the preparation method according to any one of claims 1 to 5.

7. The carbon-coated fly ash hollow microsphere thermal insulation filler according to claim 6, It is characterized in that The carbon-coated fly ash hollow microbead thermal insulation filler has a particle size between 40 and 100 um and a thermal insulation coefficient of 0.068 W / mK.

Citation Information

Cited By

  • Multifunctional super-hydrophobic insulating coating based on cavity microspheres and preparation method and application thereof