Water-based environment-friendly coating and preparation process thereof

By combining modified glass flakes and nano-titanium dioxide, the problem of easy damage to the coating caused by the high brittleness of glass flakes is solved, and the corrosion resistance and impermeability of water-based coatings are improved.

CN118994981AActive Publication Date: 2024-11-22ANHUI KAILIN ADVANCED MATERIAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411257542.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-22
Estimated Expiration
2044-09-09

AI Technical Summary

Technical Problem

Existing water-based acrylic anti-corrosion coatings contain brittle glass flakes that are easily damaged by mechanical forces, leading to surface breakage and peeling, which affects coating quality.

Method used

Modified glass flakes and modified nano-titanium dioxide were used. By depositing a boron nitride layer on the surface of the glass flakes and treating it with a silane coupling agent, the dispersibility and compatibility with the matrix of the glass flakes in acrylic emulsion were improved, forming a dense impermeable layer.

Benefits of technology

It improves the coating's corrosion resistance and impermeability, and enhances the coating's impact resistance and corrosion resistance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of water-based coatings, in particular to a water-based environment-friendly coating and a preparation process thereof.The preparation process includes the steps that water-based acrylic emulsion, deionized water, modified glass flakes and modified nano titanium dioxide are poured into a dispersion machine to be evenly stirred, and a mixture is obtained; and adding the dispersing agent, the defoaming agent, the thickening agent and the coalescing agent into the mixture, and continuously stirring uniformly to obtain the water-based environment-friendly coating. The boron nitride particle layer is deposited on the surface of the glass flake, so that the glass flake is covered and enhanced, and the problems that the glass flake is high in brittleness and not resistant to impact are solved; and then the silane coupling agent is utilized to modify the surface of the glass flake, so that the glass flake can be better dispersed in the acrylic emulsion, the compatibility of the modified glass flake and an emulsion matrix is improved, and the quality of the final coating is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of water-based coatings, in particular to a water-based environmentally friendly coating and a preparation process thereof. Background Art

[0002] Water-based environmentally friendly paint is a paint that uses water as a diluent and does not contain organic solvents. This type of paint is often non-toxic, has no irritating odor, does not pollute the environment, has a full paint film, and is easy to use. Among them, water-based acrylic anti-corrosion paint has a good application in the fields of metal, furniture, and automobiles.

[0003] Some water-based acrylic anti-corrosion coatings use glass flakes as anti-corrosion fillers. The core principle is that glass flakes can form a unique shielding protection structure in the coating, isolating the corrosive medium from the substrate, preventing the corrosive medium from penetrating the coating, and thus reducing the erosion of the substrate by corrosive substances. However, glass flakes themselves are brittle and susceptible to mechanical damage. When the formed coating is impacted by external forces, the internal glass flakes will break, causing the coating surface to be easily damaged and peeled off, which seriously affects the quality of water-based acrylic anti-corrosion coatings. Summary of the invention

[0004] In order to overcome the deficiencies of the prior art, the present invention provides a water-based environmentally friendly coating and a preparation process thereof, and improves the corrosion resistance of the coating by using modified glass flakes and modified nano titanium dioxide in combination.

[0005] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a water-based environmentally friendly paint, comprising the following raw materials in parts by weight: 60-70 parts of water-based acrylic emulsion, 15-25 parts of modified glass flakes, 5-10 parts of modified nano titanium dioxide, 0.5-1 part of dispersant, 0.2-0.5 part of defoaming agent, 0.5-0.8 part of thickener, 0.5-1 part of film-forming aid, and 10-15 parts of deionized water.

[0006] Preferably, the solid content of the aqueous acrylic emulsion is 60%; the dispersant is a BYK-190 dispersant or a BYK-110 dispersant; and the defoamer is a TEGO810 defoamer or a TEGO960W defoamer.

[0007] Preferably, the thickener is BASF Rheovis AS1130 or BASF Rheovis AS1125; the film-forming aid is ethylene glycol ethyl ether or propylene glycol phenyl ether.

[0008] Preferably, the preparation method of the modified glass flakes is as follows: S1, ultrasonically clean and dry the glass flakes, and then put them into a deposition furnace; S2, introduce nitrogen, boron trichloride and ammonia into the deposition furnace for deposition reaction, and after the deposition reaction is completed, cool to room temperature with the furnace to obtain pretreated glass flakes;

[0009] S3. Use a silane coupling agent to coat the surface of the pretreated glass flakes to obtain modified glass flakes.

[0010] Preferably, in step S1, the size of the glass flakes is 100-200 μm.

[0011] Preferably, in step S2, the specific process of the deposition reaction is as follows: the flow ratio of nitrogen, boron trichloride and ammonia is 50:10:1, the deposition reaction pressure is 45 mbar, the deposition reaction temperature is 750°C, and the deposition reaction time is 4 hours.

[0012] Preferably, the modified nano-titanium dioxide is coated on the surface of the nano-titanium dioxide using a silane coupling agent.

[0013] Preferably, the silane coupling agent is any one or more combinations of silane coupling agent KH-550, silane coupling agent KH-560, and silane coupling agent KH-570.

[0014] The present invention also provides a preparation process of a water-based environmentally friendly coating, comprising the following steps:

[0015] (1) pouring water-based acrylic emulsion, deionized water, modified glass flakes and modified nano-titanium dioxide into a disperser and uniformly stirring to obtain a mixture;

[0016] (2) Add dispersant, defoamer, thickener and film-forming aid to the mixture, continue to stir evenly, and prepare water-based environmentally friendly paint.

[0017] The present invention provides a water-based environmentally friendly coating and a preparation process thereof, which has the following beneficial effects compared with the prior art:

[0018] The present invention achieves enhanced coverage of glass flakes by depositing a boron nitride particle layer on the surface of glass flakes, thereby overcoming the problems of glass flakes being brittle and not resistant to impact. A silane coupling agent is then used to modify the surface of the glass flakes so that they can be better dispersed in an acrylic emulsion, thereby improving the compatibility of the modified glass flakes with the emulsion matrix, thereby improving the quality of the final coating.

[0019] The present invention uses modified glass flakes and modified nano titanium dioxide in combination to improve the corrosion resistance of the coating; specifically, the modified glass flakes can be arranged in parallel and overlapped with the substrate in the coating to form a dense anti-seepage layer similar to fish scales, which greatly prolongs the medium penetration path and time, and improves the anti-penetration performance and corrosion resistance of the coating; and allowing nano-scale titanium dioxide to be dispersed in the gaps between the modified glass flakes can further improve the corrosion resistance of the coating. DETAILED DESCRIPTION

[0020] The following examples are used to explain the implementation methods of the present application in detail, so that the implementation process of how the present application uses technical means to solve technical problems and achieve technical effects can be fully understood and implemented accordingly.

[0021] Example 1

[0022] The preparation method of modified glass flakes is as follows:

[0023] S1. Ultrasonic clean and dry glass flakes with a size of 100-200 μm, and then place them in a deposition furnace.

[0024] S2. Nitrogen, boron trichloride and ammonia are introduced into the deposition furnace at a flow ratio of 50:10:1 for deposition reaction. After the deposition reaction is completed, the furnace is cooled to room temperature to obtain pretreated glass flakes. During the deposition reaction, the deposition reaction pressure is 45 mbar, the deposition reaction temperature is 750°C, and the deposition reaction time is 4 hours.

[0025] S3. Use silane coupling agent KH-550 to coat the surface of the pretreated glass flakes to obtain modified glass flakes.

[0026] Example 2

[0027] The method is basically the same as Example 1, except that the silane coupling agent KH-550 is replaced by KH-560.

[0028] Example 3

[0029] The same as Example 1, except that the silane coupling agent KH-550 is replaced by KH-570

[0030] Example 4

[0031] A water-based environmentally friendly coating comprises the following raw materials in parts by weight: 70 parts of water-based acrylic emulsion with a solid content of 60%, 15 parts of modified glass flakes, 10 parts of modified nano titanium dioxide, 0.5 parts of BYK-190 dispersant, 0.5 parts of TEGO810 defoamer, 0.5 parts of BASF RheovisAS1130 thickener, 1 part of ethylene glycol ethyl ether, and 10 parts of deionized water. The surface of the modified nano titanium dioxide is coated with a silane coupling agent KH-550.

[0032] A preparation process of a water-based environmentally friendly coating comprises the following steps:

[0033] (1) pouring water-based acrylic emulsion, deionized water, modified glass flakes and modified nano-titanium dioxide into a disperser and uniformly stirring to obtain a mixture;

[0034] (2) Add dispersant, defoamer, thickener and film-forming aid to the mixture, continue to stir evenly, and prepare water-based environmentally friendly paint.

[0035] In this embodiment, the modified glass flakes in Example 1 are used.

[0036] Example 5

[0037] A water-based environmentally friendly coating comprises the following raw materials in parts by weight: 60 parts of water-based acrylic emulsion with a solid content of 60%, 25 parts of modified glass flakes, 5 parts of modified nano titanium dioxide, 1 part of BYK-110 dispersant, 0.2 parts of TEGO960W defoamer, 0.8 parts of BASF RheovisAS1125 thickener, 0.5 parts of propylene glycol phenyl ether, and 15 parts of deionized water. The surface of the modified nano titanium dioxide is coated with a silane coupling agent KH-560.

[0038] A preparation process of a water-based environmentally friendly coating comprises the following steps:

[0039] (1) pouring water-based acrylic emulsion, deionized water, modified glass flakes and modified nano-titanium dioxide into a disperser and uniformly stirring to obtain a mixture;

[0040] (2) Add dispersant, defoamer, thickener and film-forming aid to the mixture, continue to stir evenly, and prepare water-based environmentally friendly paint.

[0041] In this embodiment, the modified glass flakes in Example 2 are used.

[0042] Example 6

[0043] A water-based environmentally friendly coating comprises the following raw materials in parts by weight: 65 parts of water-based acrylic emulsion with a solid content of 60%, 20 parts of modified glass flakes, 8 parts of modified nano titanium dioxide, 0.6 parts of BYK-190 dispersant, 0.4 parts of TEGO810 defoamer, 0.6 parts of BASF RheovisAS1130 thickener, 0.8 parts of ethylene glycol ethyl ether, and 12 parts of deionized water. The surface of the modified nano titanium dioxide is coated with a silane coupling agent KH-570.

[0044] A preparation process of a water-based environmentally friendly coating comprises the following steps:

[0045] (1) pouring water-based acrylic emulsion, deionized water, modified glass flakes and modified nano-titanium dioxide into a disperser and uniformly stirring to obtain a mixture;

[0046] (2) Add dispersant, defoamer, thickener and film-forming aid to the mixture, continue to stir evenly, and prepare water-based environmentally friendly paint.

[0047] In this embodiment, the modified glass flakes in Example 3 are used.

[0048] Comparative Example 1

[0049] A water-based environmentally friendly paint comprises the following raw materials in parts by weight: 65 parts of water-based acrylic emulsion with a solid content of 60%, 20 parts of modified glass flakes, 0.6 parts of BYK-190 dispersant, 0.4 parts of TEGO 810 defoamer, 0.6 parts of BASF Rheovis AS 1130 thickener, 0.8 parts of ethylene glycol ethyl ether, and 12 parts of deionized water.

[0050] A preparation process of a water-based environmentally friendly coating comprises the following steps:

[0051] (1) pouring the aqueous acrylic emulsion, deionized water and modified glass flakes into a disperser and uniformly stirring to obtain a mixture;

[0052] (2) Add dispersant, defoamer, thickener and film-forming aid to the mixture, continue to stir evenly, and prepare water-based environmentally friendly paint.

[0053] In this comparative example, the modified glass flakes in Example 3 were used.

[0054] Comparative Example 2

[0055] Basically the same as Example 6, except that the modified glass flakes are replaced by pretreated glass flakes.

[0056] Comparative Example 3

[0057] The same as Example 6, except that: the preparation method of the modified glass flakes is as follows:

[0058] S1. Ultrasonic clean and dry glass flakes with a size of 100-200 μm, and then place them in a deposition furnace.

[0059] S2. Use silane coupling agent KH-550 to coat the surface of the cleaned glass flakes to obtain modified glass flakes.

[0060] Comparative Example 4

[0061] A water-based environmentally friendly coating comprises the following raw materials in parts by weight: 65 parts of a water-based acrylic emulsion with a solid content of 60%, 20 parts of modified glass flakes of comparative example 3, 10 parts of modified boron nitride, 8 parts of modified nano titanium dioxide, 0.6 parts of BYK-190 dispersant, 0.4 parts of TEGO810 defoamer, 0.6 parts of BASF RheovisAS1130 thickener, 0.8 parts of ethylene glycol ether, and 12 parts of deionized water. The surface of the modified nano titanium dioxide is coated with a silane coupling agent KH-570. The surface of the modified boron nitride is coated with a silane coupling agent KH-570.

[0062] A preparation process of a water-based environmentally friendly coating comprises the following steps:

[0063] (1) pouring the aqueous acrylic emulsion, deionized water, the modified glass flakes of Comparative Example 3, the modified nano titanium dioxide and the modified boron nitride into a disperser and uniformly stirring to obtain a mixture;

[0064] (2) Add dispersant, defoamer, thickener and film-forming aid to the mixture, continue to stir evenly, and prepare water-based environmentally friendly paint.

[0065] Quality Inspection

[0066] 1. The technical indicators of the water-based environmentally friendly coatings in Example 6 and Comparative Examples 1-4 were tested. The specific test results are shown in the following table.

[0067] Table 1 Coating properties

[0068] project standard Example 6 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 hardness GB6739 2H H 2H H 2H Impact resistance, cm GB / T1732 56 48 48 42 50 Salt spray resistance, h GB / T1771 735 596 558 542 627 Elongation at break, % GB / T528 621 567 537 541 588 Tensile strength, MPa GB / T528 1.45 1.28 1.27 1.21 1.34 Artificial aging, 1500h GB / T1826 Powdering Level 2 Powdering Level 2 Powdering level 3 Powdering level 3 Powdering Level 2

[0069] From the above table, we can get:

[0070] (1) Compared with Example 6, the coating in Comparative Example 1 has a weaker performance in terms of salt spray resistance, indicating that the combination of modified glass flakes / modified nano-titanium dioxide can further improve the anti-corrosion performance of the coating.

[0071] (2) The coatings in Comparative Examples 2-3 are inferior to those in Example 6 in terms of salt spray resistance, impact resistance and strength, indicating that depositing boron nitride on the surface of glass flakes and treating them with a silane coupling agent can significantly improve the quality of the coatings.

[0072] (3) Compared with Example 6, the quality of the coating in Comparative Example 4 is still slightly deviated, indicating that boron nitride deposited on glass flakes can better improve the quality of the coating.

[0073] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A water-based environmentally friendly paint, characterized in that: The invention comprises the following raw materials in parts by weight: 60-70 parts of water-based acrylic emulsion, 15-25 parts of modified glass flakes, 5-10 parts of modified nano titanium dioxide, 0.5-1 parts of dispersant, 0.2-0.5 parts of defoamer, 0.5-0.8 parts of thickener, 0.5-1 parts of film-forming aid and 10-15 parts of deionized water.

2. The water-based environmentally friendly paint according to claim 1, characterized in that: The solid content of the aqueous acrylic emulsion is 60%; the dispersant is BYK-190 dispersant or BYK-110 dispersant; and the defoamer is TEGO810 defoamer or TEGO960W defoamer.

3. The water-based environmentally friendly paint according to claim 1, characterized in that: The thickener is BASF Rheovis AS1130 or BASF Rheovis AS1125; the film-forming aid is ethylene glycol ethyl ether or propylene glycol phenyl ether.

4. The water-based environmentally friendly paint according to claim 1, characterized in that: The preparation method of the modified glass flakes is as follows: S1, ultrasonically clean and dry the glass flakes, and then place them in a deposition furnace; S2, introducing nitrogen, boron trichloride and ammonia into the deposition furnace for deposition reaction, and after the deposition reaction is completed, cooling the furnace to room temperature to obtain pretreated glass flakes; S3. Use a silane coupling agent to coat the surface of the pretreated glass flakes to obtain modified glass flakes.

5. The water-based environmentally friendly paint according to claim 4, characterized in that: In step S1, the size of the glass flakes is 100-200 μm.

6. The water-based environmentally friendly paint according to claim 4, characterized in that: In step S2, the specific process of the deposition reaction is as follows: the flow ratio of nitrogen, boron trichloride and ammonia is 50:10:1, the deposition reaction pressure is 45 mbar, the deposition reaction temperature is 750°C, and the deposition reaction time is 4 hours.

7. The water-based environmentally friendly paint according to claim 1, characterized in that: The modified nano titanium dioxide is prepared by coating the surface of the nano titanium dioxide with a silane coupling agent.

8. The water-based environmentally friendly paint according to claim 4 or 7, characterized in that: The silane coupling agent is any one or more combinations of silane coupling agent KH-550, silane coupling agent KH-560, and silane coupling agent KH-570.

9. The process for preparing the water-based environmentally friendly coating according to any one of claims 1 to 8, characterized in that: The following steps are involved: (1) pouring water-based acrylic emulsion, deionized water, modified glass flakes and modified nano-titanium dioxide into a disperser and uniformly stirring to obtain a mixture; (2) Add dispersant, defoamer, thickener and film-forming aid to the mixture, continue to stir evenly, and prepare water-based environmentally friendly paint.

Citation Information

Patent Citations

  • Interference pigments on the basis of glass flakes

    CN101203574A

  • Glass flake coating

    CN107286846A

  • Preparation method of solvent-free epoxy glass flake coating

    CN109836963A

  • Composite material modified wear-resistant and corrosion-resistant coating as well as preparation method thereof

    CN110527404A

  • Anticorrosive antifouling antistatic coating and preparation method thereof

    CN115678409A